Preparation method of ferroelectric capacitor
Through hard mask technology, ensure the uniformity and integrity of the lower electrode layer in the preparation of ferroelectric capacitors, solve the problem of electrical instability caused by maskless etching, simplify the process and reduce costs, and avoid yellow photoetching. The damage to the capacitor hole achieves more stable capacitance performance.
Patent Information
- Application Number
- CN202411038088.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing ferroelectric capacitor preparation process, the use of maskless etching makes it difficult to control the uniformity of the lower electrode layer, resulting in unstable electrical properties, and the yellow photoetching process may damage the capacitor holes and affect the performance of the capacitor.
Using hard mask technology, plasma etching is performed on the lower electrode surface to ensure the integrity and uniformity of the lower electrode layer, and deposition of ferroelectric film and upper electrode without using yellow photoetching process to simplify preparation Process to avoid damage to the capacitor hole.
The uniformity of the lower electrode layer is improved, production costs are reduced, ALD process time is shortened, maskless etching is avoided to consume the lower electrode layer, short circuit risk is reduced, and capacitor stability is improved.
Smart Images

Figure CN118946258A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of storage and relates to a method for preparing a ferroelectric capacitor. Background Art
[0002] The order of preparing ferroelectric capacitors in the existing process is as follows: capacitor hole preparation → isolation layer deposition (tantalum nitride) → bottom electrode plate (TiN, titanium nitride) → lower electrode etching (maskless dry etching) → high dielectric material deposition (high-K material ALD atomic layer deposition, in the present invention, doped hafnium oxide is used as a ferroelectric storage medium) → upper electrode plate deposition (TiN, titanium nitride) → plate line deposition → plate line photolithography & etching → high dielectric material etching. The lower electrode etching adopts maskless etching, which mainly utilizes the etching micro-load effect (the number of reaction gas molecules per unit area is the same, and the deep hole is equivalent to increasing the etching area, so the etching rate in the deep hole is much smaller than the etching rate on the wafer surface at the same position, so as to achieve the purpose of etching the wafer surface and retaining the film layer in the hole). During the dry etching process, although the etching speed of the film in the cell hole is slow, it will also be thinned.
[0003] The uniformity of the lower electrode etched without mask and the amount retained at the top of the cell hole are difficult to control, which will cause a certain difference in the area of the electrode plate of each cell, resulting in electrical instability (according to the capacitance formula C = εA / d, ε is the dielectric capacitance constant, which is determined by the material itself; A represents the area of parallel plates, d represents the distance between parallel plates (i.e., dielectric thickness), and the upper and lower electrode plates are A in the formula). Summary of the invention
[0004] In order to solve the technical problems existing in the prior art, the present invention provides a method for preparing a ferroelectric capacitor. The preparation method does not use yellow light etching process, avoids damage to the capacitor holes during the preparation process, improves the uniformity of the capacitor, and simplifies the preparation process.
[0005] In order to achieve the above technical effects, the present invention adopts the following technical solutions:
[0006] The present invention provides a method for preparing a ferroelectric capacitor, the method comprising:
[0007] A unit hole is prepared on one side of the wafer, and a barrier layer and a lower electrode are deposited in sequence on one side of the unit hole;
[0008] A hard mask is prepared on the surface of the lower electrode, the hard mask is plasma-etched to the surface of the lower electrode, and the lower electrode layer and the barrier layer are etched;
[0009] The hard mask is removed, and ferroelectric thin film deposition, upper electrode deposition, plate line preparation and ferroelectric dielectric etching are sequentially performed on the lower electrode side to obtain a ferroelectric capacitor.
[0010] As a preferred technical solution of the present invention, the thickness of the hard mask is 500-1000nm, and the unit hole is completely filled. The thickness of the hard mask can be 500nm, 550nm, 600nm, 650nm, 700nm, 750nm, 800nm, 850nm, 900nm, 950nm or 1000nm, but is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0011] As a preferred technical solution of the present invention, the method for preparing the hard mask includes spin coating.
[0012] As a preferred technical solution of the present invention, the spin coating rotation speed is 2500-3000rpm, such as 2500rpm, 2600rpm, 2700rpm, 2800rpm, 2900rpm or 3000rpm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0013] As a preferred technical solution of the present invention, the material of the hard mask includes carbon-containing organic matter, and the solid content of the hard mask is greater than 45%, such as 46%, 48%, 50%, 55%, 60%, 65%, 70% or 75%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0014] As a preferred technical solution of the present invention, the hard mask is plasma etched to the surface of the lower electrode and the unit opening.
[0015] As a preferred technical solution of the present invention, the ferroelectric thin film layer is a Zr-doped hafnium oxide thin film.
[0016] As a preferred technical solution of the present invention, the thickness of the ferroelectric thin film layer is 8 to 10 nm, such as 8 nm, 8.2 nm, 8.5 nm, 8.8 nm, 9 nm, 9.2 nm, 9.5 nm, 9.8 nm or 10 nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0017] As a preferred technical solution of the present invention, the method for preparing the ferroelectric thin film layer includes atomic layer deposition.
[0018] As a preferred technical solution of the present invention, annealing treatment is performed after deposition of the ferroelectric thin film and the upper electrode, and the annealing temperature is 500-600°C, such as 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C or 600°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0019] Compared with the prior art, the present invention has at least the following beneficial effects:
[0020] (1) The present invention provides a method for preparing a ferroelectric capacitor. The method does not use yellow light photolithography. By using a hard mask, the consumption of the lower electrode layer in the capacitor hole by maskless etching is avoided. The thickness of the titanium nitride of the lower electrode can be reduced from 15 nm to 10 nm, thereby reducing the production cost and shortening the ALD (atomic layer deposition) process time.
[0021] (2) The present invention provides a method for preparing a ferroelectric capacitor. The method ensures the integrity of the lower electrode layer and improves the uniformity of the lower electrode layer by using a hard mask. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 A schematic flow chart of a method for preparing a ferroelectric capacitor provided in Example 1;
[0023] In the figure: 1-blocking layer, 2-lower electrode layer, 3-hard mask layer, 4-ferroelectric thin film, 5-upper electrode layer.
[0024] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION
[0025] The technical solution of the present application is further described below through specific implementation methods.
[0026] The specific embodiment of the present application provides a method for preparing a ferroelectric capacitor, the preparation method comprising:
[0027] A unit hole is prepared on one side of the wafer, and a barrier layer and a lower electrode are deposited in sequence on one side of the unit hole;
[0028] A hard mask is prepared on the surface of the lower electrode, the hard mask is plasma-etched to the surface of the lower electrode, and the lower electrode layer and the barrier layer are etched;
[0029] The hard mask is removed, and ferroelectric thin film deposition, upper electrode deposition, plate line preparation and ferroelectric dielectric etching are sequentially performed on the lower electrode side to obtain a ferroelectric capacitor.
[0030] In the present invention, the use of a hard mask and plasma etching of the hard mask not only simplifies the process (reducing the photolithography process), but also, due to the difference in etching rate, there will be a certain amount of over-etching at the top of the deep hole, and the lower electrode is 50 to 100 nm lower than the side wall of the capacitor hole, avoiding the risk of short circuit caused by the lower electrodes being too close due to the smaller hole spacing after the capacitor hole density is further increased.
[0031] In a specific embodiment of the present invention, the method for preparing the capacitor hole can be to deposit a silicon nitride + silicon oxide + silicon nitride + silicon oxide + silicon nitride structure in sequence on a wafer on which transistor pole winding has been completed, and use yellow light + dry etching to prepare the capacitor hole on the silicon nitride + silicon oxide + silicon nitride + silicon oxide + silicon nitride structure.
[0032] In a specific embodiment of the present invention, the thickness of the silicon nitride layer in the silicon nitride + silicon oxide + silicon nitride + silicon oxide + silicon nitride structure can be 30 to 50 nm, the thickness of the silicon oxide layer can be 500 to 1000 nm, and the thickness of the top silicon nitride is 100 to 200 nm.
[0033] In a specific embodiment of the present invention, the capacitor hole may have a diameter of 150-200 nm and a depth of 1000-1500 nm.
[0034] In a specific embodiment of the present invention, the barrier layer may be prepared by physical vapor deposition.
[0035] In a specific embodiment of the present invention, the material of the barrier layer is preferably tantalum nitride, which serves as a metal barrier layer to prevent metal from diffusing in the dielectric layer.
[0036] In a specific embodiment of the present invention, the thickness of the barrier layer may be 10 to 15 nm.
[0037] In a specific embodiment of the present invention, the lower electrode layer may be prepared by atomic layer deposition.
[0038] In a specific embodiment of the present invention, the material of the lower electrode layer is preferably titanium nitride.
[0039] In a specific embodiment of the present invention, the thickness of the lower electrode layer may be 10 to 15 nm.
[0040] In a specific embodiment of the present invention, the material of the hard mask can be a high-carbon polymer, such as spin-on carbon.
[0041] In a specific embodiment of the present invention, the hard mask is cured after spin coating, and the curing temperature and time can be specifically selected according to the material of the hard mask, and are not further limited herein.
[0042] In a specific embodiment of the present invention, the electrode layer and the barrier layer on the surface of the top silicon nitride layer may be removed by dry etching, and the reaction gas may be chlorine or hydrogen bromide.
[0043] In a specific embodiment of the present invention, the hard mask layer inside the capacitor hole may be removed by dry etching, more preferably oxygen plasma etching, and the etching stops at the surface of the lower electrode layer.
[0044] In a specific embodiment of the present invention, the ferroelectric thin film layer may be prepared by atomic layer deposition.
[0045] In a specific embodiment of the present invention, the material of the ferroelectric thin film layer is Zr-doped HfO2, preferably Hf 1- x Zr x O2, 0<x<1; more preferably Hf 0.5 Zr 0.5 O2.
[0046] In a specific embodiment of the present invention, the upper electrode layer may be prepared by atomic layer deposition.
[0047] In a specific embodiment of the present invention, the material of the upper electrode layer is preferably titanium nitride.
[0048] In a specific embodiment of the present invention, the thickness of the upper electrode layer may be 10 to 15 nm.
[0049] In one embodiment of the present invention, annealing is used to transform the T phase (non-ferroelectric) in Zr-doped HfO2 into the O phase (ferroelectric phase), thereby increasing the residual polarity and obtaining a stable ferroelectric capacitor structure.
[0050] In a specific embodiment of the present invention, the method of preparing the plate line includes physical vapor deposition of a layer of metal Ti or Al with a thickness of 200 to 300 nm, and filling the capacitor holes; through yellow light and dry etching process, only the metal layer in the storage array area is retained, and all other areas are removed.
[0051] In a specific embodiment of the present invention, the ferroelectric dielectric etching method can be dry etching, and the etching gas can be perfluoromethane or octafluorocyclobutane to completely remove the ferroelectric film in the exposed area (area without plate line pattern protection).
[0052] In a specific embodiment of the present invention, the specific conditions of processes such as physical vapor deposition, atomic layer deposition, yellow light lithography, dry etching and plasma etching used in the ferroelectric capacitor preparation method can be specifically selected according to the thickness and material of the corresponding preparation layer or etching layer, and are not further limited here.
[0053] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0054] Example 1
[0055] This embodiment provides a method for preparing a ferroelectric capacitor, the process of which is as follows: Figure 1 As shown, the preparation method comprises:
[0056] (1) On a wafer that has completed transistor pole winding, a structure of silicon nitride + silicon oxide + silicon nitride + silicon oxide + silicon nitride is sequentially deposited, with a silicon nitride layer having a thickness of 30 nm, a silicon oxide layer having a thickness of 500 nm, and a top silicon nitride layer having a thickness of 200 nm; yellow light + dry etching is used to prepare capacitor holes, with a hole diameter of 150 nm and a depth of 1000 nm;
[0057] (2) depositing tantalum nitride as a barrier layer by physical vapor deposition with a thickness of 10 nm;
[0058] (3) depositing titanium nitride as a lower electrode layer on the barrier layer by atomic layer deposition with a thickness of 10 nm;
[0059] (4) Spin coating an organic carbon silicon solution as a hard mask layer at a rotation speed of 2500 rpm and a thickness of 500 nm to fill the capacitor holes, and cure the hard mask layer at 300°C for 60 min;
[0060] (5) etching the hard mask layer with oxygen-containing plasma to the surface of the lower electrode layer;
[0061] (6) using a dry etching process (with Cl2 and HBr as the reaction gas) to remove the lower electrode layer and the barrier layer on the surface of the top silicon nitride layer;
[0062] (7) using oxygen-containing plasma etching to remove the hard mask layer inside the capacitor hole;
[0063] (8) Atomic layer deposition is used to deposit a ferroelectric thin film layer made of Hf 0.5 Zr 0.5 O2, thickness 8nm;
[0064] (9) A titanium nitride layer is deposited as the upper electrode layer by atomic layer deposition, with a thickness of 10 nm;
[0065] (10) Annealing the structure after depositing the upper electrode layer at a temperature of 500° C.
[0066] (11) Physical vapor deposition is used to deposit a layer of Ti with a thickness of 200 nm to fill the capacitor holes;
[0067] (12) Using yellow light + dry etching, only the metal layer in the storage array area is retained, and all other areas are removed;
[0068] (13) Dry etching is performed using tetrafluoromethane as etching gas to completely remove the ferroelectric film in the exposed area (area without line pattern protection).
[0069] Example 2
[0070] This embodiment provides a method for preparing a ferroelectric capacitor, the method comprising:
[0071] (1) On a wafer on which transistor pole winding has been completed, a structure of silicon nitride + silicon oxide + silicon nitride + silicon oxide + silicon nitride is sequentially deposited, with a silicon nitride layer having a thickness of 50 nm, a silicon oxide layer having a thickness of 1000 nm, and a top silicon nitride layer having a thickness of 100 nm; yellow light + dry etching is used to prepare capacitor holes with a hole diameter of 200 nm and a depth of 1500 nm;
[0072] (2) depositing tantalum nitride as a barrier layer by physical vapor deposition with a thickness of 15 nm;
[0073] (3) depositing titanium nitride as a lower electrode layer on the barrier layer by atomic layer deposition with a thickness of 10 nm;
[0074] (4) Spin coating an organic carbon silicon solution as a hard mask layer at a rotation speed of 3000 rpm and a thickness of 1000 nm to fill the capacitor holes, and curing the hard mask layer at 300° C. for 60 min;
[0075] (5) etching the hard mask layer with oxygen-containing plasma to the surface of the lower electrode layer;
[0076] (6) using a dry etching process (with Cl2 and HBr as the reaction gas) to remove the lower electrode layer and the barrier layer on the surface of the top silicon nitride layer;
[0077] (7) using oxygen-containing plasma etching to remove the hard mask layer inside the capacitor hole;
[0078] (8) Atomic layer deposition is used to deposit a ferroelectric thin film layer made of Hf 0.8 Zr 0.2 O2, thickness 10nm;
[0079] (9) A titanium nitride layer is deposited as the upper electrode layer by atomic layer deposition, with a thickness of 15 nm;
[0080] (10) Annealing the structure after depositing the upper electrode layer at a temperature of 600° C.
[0081] (11) Physical vapor deposition is used to deposit a layer of Al with a thickness of 300 nm to fill the capacitor holes;
[0082] (12) Using yellow light + dry etching, only the metal layer in the storage array area is retained, and all other areas are removed;
[0083] (13) Dry etching is performed using octafluorocyclobutane as etching gas to completely remove the ferroelectric film in the exposed area (area without line pattern protection).
[0084] Example 3
[0085] This embodiment provides a method for preparing a ferroelectric capacitor, the method comprising:
[0086] (1) On a wafer that has completed transistor pole winding, a structure of silicon nitride + silicon oxide + silicon nitride + silicon oxide + silicon nitride is sequentially deposited, with a silicon nitride layer having a thickness of 40 nm, a silicon oxide layer having a thickness of 600 nm, and a top silicon nitride layer having a thickness of 120 nm; a capacitor hole is prepared by yellow light + dry etching, with a hole diameter of 160 nm and a depth of 1200 nm;
[0087] (2) depositing tantalum nitride as a barrier layer by physical vapor deposition with a thickness of 12 nm;
[0088] (3) depositing titanium nitride as a lower electrode layer on the barrier layer by atomic layer deposition with a thickness of 10 nm;
[0089] (4) Spin coating an organic carbon silicon solution as a hard mask layer at a rotation speed of 2700 rpm and a thickness of 700 nm to fill the capacitor holes, and cure the hard mask layer at 300° C. for 60 min;
[0090] (5) etching the hard mask layer with oxygen-containing plasma to the surface of the lower electrode layer;
[0091] (6) using a dry etching process (with Cl2 and HBr as the reaction gas) to remove the lower electrode layer and the barrier layer on the surface of the top silicon nitride layer;
[0092] (7) using oxygen-containing plasma etching to remove the hard mask layer inside the capacitor hole;
[0093] (8) Atomic layer deposition is used to deposit a ferroelectric thin film layer made of Hf 0.6 Zr 0.4 O2, thickness 10nm;
[0094] (9) A titanium nitride layer is deposited as the upper electrode layer by atomic layer deposition, with a thickness of 12 nm;
[0095] (10) Annealing the structure after depositing the upper electrode layer at a temperature of 550° C.
[0096] (11) Physical vapor deposition is used to deposit a layer of Ti with a thickness of 250 nm to fill the capacitor holes;
[0097] (12) Using yellow light + dry etching, only the metal layer in the storage array area is retained, and all other areas are removed;
[0098] (13) Dry etching is performed using tetrafluoromethane as etching gas to completely remove the ferroelectric film in the exposed area (area without line pattern protection).
[0099] Example 4
[0100] This embodiment provides a method for preparing a ferroelectric capacitor, the method comprising:
[0101] (1) On the wafer on which the transistor pole winding has been completed, a silicon nitride + silicon oxide + silicon nitride + silicon oxide + silicon nitride structure is sequentially deposited, the thickness of the silicon nitride layer is 45nm, the thickness of the silicon oxide layer is 800nm, and the thickness of the top silicon nitride is 150nm; yellow light + dry etching is used to prepare capacitor holes with a hole diameter of 180nm and a depth of 1250nm;
[0102] (2) depositing tantalum nitride as a barrier layer by physical vapor deposition with a thickness of 14 nm;
[0103] (3) depositing titanium nitride as a lower electrode layer on the barrier layer by atomic layer deposition with a thickness of 10 nm;
[0104] (4) Spin coating an organic carbon silicon solution as a hard mask layer at a rotation speed of 2800 rpm with a thickness of 800 nm to fill the capacitor holes, and curing the hard mask layer at 300° C. for 60 min;
[0105] (5) etching the hard mask layer with oxygen-containing plasma to the surface of the lower electrode layer;
[0106] (6) using a dry etching process (with Cl2 and HBr as the reaction gas) to remove the lower electrode layer and the barrier layer on the surface of the top silicon nitride layer;
[0107] (7) using oxygen-containing plasma etching to remove the hard mask layer inside the capacitor hole;
[0108] (8) Atomic layer deposition is used to deposit a ferroelectric thin film layer made of Hf 0.7 Zr 0.3 O2, thickness 9nm;
[0109] (9) A titanium nitride layer is deposited as the upper electrode layer by atomic layer deposition, with a thickness of 14 nm;
[0110] (10) Annealing the structure after depositing the upper electrode layer at a temperature of 550° C.
[0111] (11) Physical vapor deposition is used to deposit a layer of Ti with a thickness of 280 nm to fill the capacitor holes;
[0112] (12) Using yellow light + dry etching, only the metal layer in the storage array area is retained, and all other areas are removed;
[0113] (13) Dry etching is performed using tetrafluoromethane as etching gas to completely remove the ferroelectric film in the exposed area (area without line pattern protection).
[0114] Comparative Example 1
[0115] After the hard mask layer is prepared in step (4) of this comparative example, a photoresist is coated on the surface of the hard mask layer. The photoresist thickness is 430 nm, and the photoresist is patterned using a yellow light process, that is, a photoresist with the same area as the opening of the capacitor hole is retained above the capacitor hole; the contents of steps (1)-(3) and (5)-(13) are the same as those in Example 4.
[0116] Comparative Example 2
[0117] This comparative example provides a method for preparing a ferroelectric capacitor, the preparation method comprising:
[0118] (1) Preparation of capacitor holes, that is, depositing silicon nitride + silicon oxide + silicon nitride + silicon oxide + silicon nitride structure in sequence on the wafer that has completed transistor pole winding, where the thickness of silicon nitride is 50nm, and the thickness of silicon oxide determines the capacitor area, and its thickness is 1000nm. Then, use yellow light + dry etching to punch cylindrical holes in the node layer structure for making embedded ferroelectric capacitors, with an aperture of 200nm (aperture affects capacitance, and the bottom of the hole exceeding 200nm will be thinned more during maskless etching), and the overall capacitor hole depth is 2000nm;
[0119] (2) Barrier layer deposition, which uses atomic layer deposition to deposit a tantalum nitride film as a metal barrier layer to prevent metal diffusion in the dielectric layer, with a thickness of 15 nm;
[0120] (3) Deposition of the lower electrode plate: A layer of titanium nitride is deposited on the barrier layer by atomic layer deposition as the lower electrode plate of the capacitor, with a thickness of 15 nm;
[0121] (4) etching the lower electrode plate by plasma gas etching, taking advantage of the difference in etching speed between the wafer surface and the capacitor hole caused by the etching load effect, to achieve TiN on the wafer surface and tantalum nitride as the barrier layer, while retaining the thin film in the capacitor hole;
[0122] (5) Ferroelectric thin film deposition: hafnium oxide-based ferroelectric thin films (Hf 0.5 Zr 0.5 O2), the thickness of the ferroelectric film is 10nm;
[0123] (6) The ferroelectric thin film etching, i.e., using a dry etching method, using plasma + etching gas CF4, etc., utilizing the etching rate difference caused by the dry etching micro-load effect and the incomplete etching process, removes the ferroelectric thin film on the surface of the wafer, and the thin film in the capacitor hole is partially retained;
[0124] (7) Deposition of the upper electrode plate, i.e., using atomic layer deposition to deposit a layer of titanium nitride on the barrier layer as the upper electrode plate of the capacitor, with a thickness of 15 nm;
[0125] (8) Filling the upper electrode: using physical vapor deposition, a layer of metal Ti with a thickness of 300 nm is deposited to fill the cell hole. At this time, the ferroelectric capacitor is completed;
[0126] (9) The high temperature annealing process is to use a high temperature furnace and heat to 500° C. to obtain a ferroelectric capacitor.
[0127] The preparation method of the ferroelectric capacitor provided in Examples 1-4, by using a hard mask, avoids the consumption of the lower electrode layer in the capacitor hole by maskless etching compared with Comparative Example 2, and the thickness of the titanium nitride of the lower electrode can be reduced from 15nm to 10nm, which reduces the production cost and shortens the ALD (atomic layer deposition) process time. Compared with Comparative Example 1, since the hard mask is etched after patterning with a photoresist mask in Comparative Example 1, the remaining hard mask layer is higher than a certain height of the top opening of the capacitor hole, so that after etching the lower electrode layer and the barrier layer, the height of the lower electrode layer at the top opening of the capacitor port is flush with the top of the capacitor hole, and when the density of the capacitor holes is large, a short circuit risk is prone to occur. However, due to the difference in etching rate, the preparation method of the ferroelectric capacitor provided in Examples 1-4 will have a certain amount of over-etching at the top of the capacitor hole, and the lower electrode is 50 to 100nm lower than the side wall of the capacitor hole, which avoids the short circuit risk caused by the small hole spacing after the density of the capacitor holes is further increased.
[0128] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0129] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0130] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0131] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a ferroelectric capacitor, It is characterized in that The preparation method comprises: A unit hole is prepared on one side of the wafer, and a barrier layer and a lower electrode are deposited in sequence on the side of the unit hole; Prepare a hard mask on the surface of the lower electrode, perform plasma etching on the hard mask to the surface of the lower electrode, and etch the lower electrode layer and the barrier layer; The hard mask is removed, and ferroelectric thin film deposition, upper electrode deposition, plate line preparation and ferroelectric dielectric etching are sequentially performed on one side of the lower electrode to obtain the ferroelectric capacitor.
2. The preparation method according to claim 1, It is characterized in that The hard mask has a thickness of 500-1000 nm and completely fills the unit hole.
3. The preparation method according to claim 1, It is characterized in that The method for preparing the hard mask includes spin coating.
4. The preparation method according to claim 1, It is characterized in that The rotation speed of the spin coating is 2500-3000 rpm.
5. The preparation method according to claim 1, It is characterized in that The material of the hard mask includes carbon-containing organic matter, and the solid content of the hard mask is greater than 45%.
6. The preparation method according to claim 1, It is characterized in that The plasma etches the hard mask to the surface of the lower electrode and the unit opening.
7. The preparation method according to claim 1, It is characterized in that The ferroelectric thin film layer is a Zr-doped hafnium oxide thin film.
8. The preparation method according to claim 1, It is characterized in that The thickness of the ferroelectric thin film layer is 8-10 nm.
9. The preparation method according to claim 1, It is characterized in that The method for preparing the ferroelectric thin film layer comprises atomic layer deposition.
10. The preparation method according to claim 1, It is characterized in that After the ferroelectric thin film is deposited and the upper electrode is deposited, an annealing treatment is performed, and the temperature of the annealing treatment is 500-600°C.