Method for producing tantalum powder by reducing potassium fluotantalate with sodium and prepared tantalum powder
By preheating sodium metal and controlling the particle morphology and specific surface area of tantalum powder, the specific capacitance and breakdown voltage problems of tantalum powder preparation under high voltage empowerment conditions were solved, and a higher capacitance was achieved performance.
Patent Information
- Application Number
- CN202480001174.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-06-18
AI Technical Summary
The existing sodium reducing potassium fluorotantalate method for preparing tantalum powder has problems such as low specific capacitance, large leakage current and low breakdown voltage under high voltage empowerment conditions, which limits the performance improvement of tantalum capacitors.
Reduction is carried out by preheating to 180-350℃. Combined with the existing refinement technology, the particle morphology and specific surface area of the tantalum powder are controlled by adding potassium fluorotantalate and sodium metal, and water pickling is carried out , sintering and oxygen reduction treatment to prepare tantalum powder with a porous structure.
It significantly improves the specific capacitance and breakdown voltage of tantalum powder, and is suitable for the manufacturing of high-reliability tantalum capacitors, enhancing the voltage withstand performance of the capacitor.
Smart Images

Figure CN118946421A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of smelting rare metal functional materials, and in particular relates to tantalum powder for making high-voltage and high-reliability capacitors and a manufacturing method thereof. Background Art
[0002] Tantalum electrolytic capacitors (hereinafter referred to as tantalum capacitors) have the advantages of high capacity, small size, strong self-healing ability, and high reliability. They are widely used in high-end technical fields such as communications, computers, automotive electronics, medical equipment, radar, aerospace, and automatic control devices. Tantalum powder is the key material for making tantalum capacitors. Only by using tantalum powder for capacitors with high specific capacitance and higher voltage resistance can tantalum capacitors with smaller size and better reliability be produced. Therefore, only by continuously developing tantalum powder for capacitors with higher specific capacitance and voltage resistance can the tantalum capacitors produced continue to meet the requirements of electronic devices and electronic circuits for the miniaturization and high reliability of tantalum capacitors.
[0003] At present, the main methods for industrial preparation of capacitor-grade tantalum powder are sodium reduction potassium fluorotantalate method and magnesium reduction tantalum oxide method. The magnesium reduction tantalum oxide method is expected to produce tantalum powder for capacitors with improved specific capacitance and pressure resistance due to the change of the state of the reactants. However, due to the immature process, magnesium reduction tantalum powder has the problems of low production efficiency and high cost, which limits its promotion and application. Although the sodium reduction potassium fluorotantalate method for preparing tantalum powder has the problems of low specific capacitance, large leakage current and low breakdown voltage under relatively high voltage empowerment conditions, the sodium reduction potassium fluorotantalate method has achieved large-scale production due to its mature process and relatively low production cost. In addition, the sodium reduction potassium fluorotantalate method can easily prepare high specific capacitance tantalum powder. Therefore, sodium reduction tantalum powder currently accounts for more than 80% of the tantalum powder market for capacitors. It is of great significance to scientifically improve the problems of low specific capacitance, large leakage current and low breakdown voltage of sodium reduction tantalum powder under high voltage empowerment conditions.
[0004] In order to improve the quality of sodium reduced tantalum powder, many studies have been conducted in the industry.
[0005] US4684399A discloses a method for producing tantalum powder by reducing potassium fluorotantalate with sodium. Potassium fluorotantalate and metallic sodium are continuously or semi-continuously added to a molten diluent for stirring and reduction to obtain tantalum powder. US4149876A proposes a method for producing tantalum powder by adding liquid sodium to a molten salt bath of molten potassium fluorotantalate and diluent. The method is to rapidly inject sodium at a relatively low sodium injection temperature to raise the material temperature, use a large diluent ratio, force cooling, carry out a reduction reaction at a relatively low temperature, and maintain a constant temperature during the grain growth period, thereby producing tantalum powder with fine and uniform particle size. The patent also focuses on the reduction temperature, heating rate, and forced cooling.
[0006] CN1069564C discloses a reduction process in which phosphorus, boron, nitrogen, oxygen, and silicon are added as additives to refine tantalum powder during the reduction process. The use of refiners can significantly increase the specific volume of tantalum powder reduced by sodium. There are also patents that propose the use of iodides or sulfates in the reduction process to improve the performance of tantalum powder.
[0007] JP4828016B2 discloses a method for producing tantalum powder by reducing potassium fluorotantalate with metallic sodium. The method comprises adding a small amount of potassium fluorotantalate to a molten diluent, then adding metallic sodium for reduction, and then adding a small amount of potassium fluorotantalate for sodium reduction. The process is repeated to achieve the reaction of potassium fluorotantalate at a low concentration. The amount of diluent salt is 40-1000 times that of potassium fluorotantalate, thereby achieving the purpose of increasing the specific capacitance of the tantalum powder. The specific capacitance of the tantalum powder produced by the method is 80000-250000 μFV / g.
[0008] CN201693181U discloses a method for achieving the reaction of dispersed metallic sodium and molten potassium tantalate by means of a sodium distributor provided at the end of a sodium injection tube; CN116100040A discloses a method for reducing potassium tantalate by jetting metallic sodium to disperse the metallic sodium, and the method produces a tantalum powder product with uniform particle size distribution and uniform particle shape distribution.
[0009] In order to improve the pressure resistance of tantalum powder produced by the sodium reduction potassium fluorotantalate method, other methods include increasing the sintering temperature and extending the sintering time of subsequent treatments. However, increasing the sintering temperature and extending the sintering time will inevitably reduce the specific capacitance of the tantalum powder.
[0010] Without being bound by general theories, the inventors have found after extensive research that there are studies on the process of reducing potassium tantalate with sodium, which involve the state, temperature, and concentration of potassium tantalate (using diluent salts such as potassium chloride, sodium chloride, and potassium fluoride to disperse potassium tantalate); involving alkali metal halides as diluent salts; involving the use of additives such as compounds containing sulfur, phosphorus, boron, nitrogen, oxygen, silicon, iodine, etc. to refine tantalum powder during the reduction process; involving the temperature and fluidity of the injected liquid metal sodium, involving the stirring and mixing during the reduction process, and involving equipment for optimizing the reduction process. However, there are studies on the process of reducing potassium tantalate with sodium, which do not involve the influence of the temperature of the liquid metal sodium before injection on the particle morphology of the metal tantalum powder during the process of reducing potassium tantalate with sodium. Summary of the invention
[0011] One object of the present invention is to provide a method for preparing tantalum powder by reducing potassium fluorotantalate with high-temperature metallic sodium. The method involves reducing potassium fluorotantalate, wherein metallic sodium preheated to more than 180°C, more preferably 200-350°C, more preferably 200-260°C, more preferably 190°C-240°C, for example 210°C, is used. The tantalum powder prepared by the method, combined with the existing tantalum powder refinement technology, can prepare tantalum powder with improved morphology (for example, coarse sintering diameter, controllable specific surface area, and porous structure). The tantalum powder prepared by the process is more suitable for making tantalum capacitors with higher reliability requirements after subsequent treatments such as existing water pickling purification, sintering, and oxygen reduction. Compared with other methods for producing tantalum powder for capacitors of the same grade, the tantalum powder has a high specific capacitance and a high breakdown voltage under high-voltage energizing conditions, which significantly improves the withstand voltage performance of tantalum powder for capacitors. In other words, tantalum powder for capacitors with different specific capacitances produced by the method of the present invention can withstand relatively higher voltages, and tantalum capacitors made using it have higher reliability.
[0012] Another object of the present invention is to provide a method for preparing tantalum powder by sodium reduction of potassium fluorotantalate, comprising the following steps:
[0013] (1) providing a diluent salt (preferably selected from alkali metal halides), potassium tantalate and metallic sodium as raw materials, wherein the amount of metallic sodium is in excess relative to the amount of potassium tantalate, and the metallic sodium is preheated to 180-350° C. (preferably 200-350° C., more preferably 200-260° C., more preferably 160-190° C. and / or 210-240° C.) for use,
[0014] (2) placing a diluted salt into a reduction container, evacuating the container, and then introducing an inert gas such as argon, and then heating the diluted salt in the reduction container until it melts while the inert gas is kept flowing (for example, at a flow rate of 20-100 liters / minute),
[0015] (3) adding a portion of potassium fluorotantalate to a reduction vessel, monitoring the temperature to ensure that the potassium fluorotantalate and the dilute salt are melted, and then adding preheated metallic sodium to reduce the portion of the potassium fluorotantalate, repeating the process multiple times until all the potassium fluorotantalate and metallic sodium raw materials are used up.
[0016] (4) After the reduction is completed, the tantalum powder is aged, and
[0017] (5) Then, the tantalum powder is separated.
[0018] Optionally, after step (5), the method further comprises the following steps:
[0019] (6) The tantalum powder is subjected to salt bath heat treatment and / or agglomeration heat treatment, the metal magnesium chips are subjected to oxygen reduction treatment, and further pickling, purification and drying are performed to obtain a tantalum powder product.
[0020] In step (1), the diluent salt is selected from alkali metal halides commonly mentioned in the prior art (also called alkali metal halogen salts, and "halide salts" and "halides" can be used interchangeably in this article), such as one or more of NaCl, KCl, KF, and KI. There is no restriction on the ratio of the diluent salt to potassium tantalate fluoroate, and the ratio commonly used in the prior art can be adopted. Preferably, tantalum powder refining agent can also be mixed in the diluent salt. The amount of metallic sodium is in excess of the theoretical amount for completely reducing potassium tantalate fluoroate, for example, an excess of 1-3%, preferably an excess of 1.5-2.5%. The metallic sodium is preheated to more than 180°C-500°C, more preferably 200-350°C, more preferably 200-260°C, more preferably 190°C-240°C, for example 210°C. Preferably, the diluent salt and potassium tantalate are both in the form of powder.
[0021] Preferably, in step (2), the evacuation and introduction of an inert gas such as argon are repeated multiple times, for example, 2-3 times, to exhaust the air in the reduction container as much as possible, reduce the corrosion of the metal reduction container by air, and reduce the adverse effects of air on tantalum powder. In order to allow the water vapor and acidic gas released during the heating and melting process to be carried by the argon gas and discharged from the reduction container in time to reduce the adverse effects on the reduction, preferably, the inert gas flow rate is maintained at 20-100 liters / minute, which can better discharge water vapor and acidic gases. In order to ensure that it is completely melted and improve the viscosity of the diluted salt so that stirring is smoother, the diluted salt is preferably heated to a temperature exceeding its melting point by 80°C, preferably exceeding 150°C, and more preferably exceeding 200°C. Preferably, after being fully melted, it is also kept warm, for example, for 30 minutes. Preferably, the diluted salt is stirred after being heated to the target temperature so as to be fully mixed and keep the temperature uniform. There are no special requirements for the stirring conditions. Preferably, after the diluted salt is melted, it is continuously stirred, preferably until the aging is completed.
[0022] In step (3), potassium fluorotantalate is added in multiple times and the reduction is completed in order to reduce the concentration of potassium fluorotantalate in the diluted salt. There is no restriction on the amount of potassium fluorotantalate added each time and the number of additions. However, after a lot of research, the inventors found that the specific amount of potassium fluorotantalate added each time is related to the target specific surface area of the final tantalum powder. In the case where a fixed amount of diluted salt has been added in step (2), if a tantalum powder with a larger specific surface area is to be prepared, the amount of potassium fluorotantalate added each time can be reduced to reduce potassium fluorotantalate at a lower concentration. If a tantalum powder with a smaller specific surface area is to be prepared, the amount of potassium fluorotantalate added each time is appropriately increased. That is to say, the present invention achieves good control of the specific surface area of tantalum powder. Of course, no matter how many times potassium fluorotantalate is added, when metallic sodium is added for the last time, all the remaining raw sodium is added to ensure that potassium fluorotantalate is completely reduced. Preferably, in this step, the temperature in the reduction container is controlled to exceed the melting point of the mixture of diluted salt and potassium fluorotantalate to ensure its melting, for example, exceeding its melting point by 80°C-400°C, preferably exceeding 250°C-350°C. It is easy for a person skilled in the art to understand that the temperature at which the mixture of the diluted salt and potassium tantalate is melted may be different from the melting point of the diluted salt and the melting point of potassium tantalate. When the ratio of the two is different, the "melting point" (also called the apparent melting point) when the mixture is completely melted is also different, but its apparent melting point can be found based on the phase diagram data. Preferably, the temperature is increased after each addition of potassium tantalate. Preferably, in order to make the obtained tantalum powder more uniform, before the last addition of metallic sodium, the amount of high-temperature metallic sodium added each time is such that 70-95%, more preferably 70-85%, of the potassium tantalate just added is reduced. This addition method can avoid the excessive metallic sodium in the reduction container from reacting with the potassium tantalate added later too early (i.e., when it is not melted).
[0023] In step (4), preferably, the tantalum powder is aged by continuing to heat and keep the tantalum powder warm after the reduction is completed. Preferably, the heating is continued for 0.5-5 hours, preferably 2-3 hours. Preferably, the temperature in the reaction vessel is controlled to be the temperature before adding the metallic sodium in step (3). In this step, the excess metallic sodium is carried away from the reduction vessel by the argon gas and separated from the tantalum powder.
[0024] Preferably, in step (3) and / or (4), an inert gas such as argon is always circulated in the reduction container. Preferably, in step (5), the reduction container is kept at a positive pressure until the mixed material is started to be taken out of the reduction container.
[0025] Preferably, separating the tantalum powder in step (5) includes: stopping stirring, cooling to room temperature while introducing argon gas to maintain a positive pressure in the reduction reaction container, taking out a mixture containing halide and tantalum powder from the reduction container, separating and removing part of the by-products that do not wrap the tantalum powder, and further separating the by-products by water acid washing, washing, purifying and drying to obtain the final tantalum powder.
[0026] Preferably, the method of the present invention further comprises step (6) after step (5): water washing and / or pickling, heat treatment such as high temperature and high vacuum heat treatment (or high temperature and high vacuum heat treatment after molten salt assisted sintering according to the invention of patent CN114210973B), oxygen reduction, pickling, and then separating the tantalum powder by filtering and drying, so as to obtain tantalum powder suitable for making high-reliability tantalum capacitors. These treatments are all known processes in the prior art. In other words, these treatments can adopt any process known in the prior art. For example, the high-temperature and high-vacuum heat treatment and passivation here can adopt the methods provided by patents CN201110039272.9, CN201120077798.1, CN201120077680.9, CN201120077305.4, etc., the oxygen reduction can adopt the methods provided by patents CN201420777210.7, CN201420777210.7, and the pickling can adopt the methods provided by patents CN201210548101.3, CN201280077499.5, CN201210548008.2, etc.
[0027] The present invention may also include adding N, P and / or B elements to the tantalum powder after step (5) and / or (6). Of course, raw materials containing these elements may also be used directly. These elements may also be added in the aforementioned high temperature and high vacuum heat treatment step. It is particularly preferred to add the P element. Adding the P element can increase the specific volume. As long as the total amount of P doping is controlled, the effect of increasing the specific volume is the same regardless of when it is added. This can be done in a conventional manner in the prior art and will not be described in detail.
[0028] The obtained tantalum powder product was pressed into blocks, sintered, and energized under high voltage conditions. The electrical properties of the energized blocks were tested, and it was found that the energized blocks had a higher specific capacitance and a higher breakdown voltage in the breakdown voltage test.
[0029] After being energized under the same high voltage conditions, the tantalum powder produced by the present invention has a higher specific capacitance than tantalum powder for capacitors of the same grade produced by other methods, and the breakdown voltage test shows a higher breakdown voltage. Therefore, the tantalum powder produced by the present invention is more suitable for making high-voltage and high-reliability tantalum capacitors.
[0030] Without being bound by general theories, the inventors believe that the reasons for the excellent effects of the present invention are as follows. The reduction of potassium fluorotantalate by sodium is a violent exothermic process, which will release a large amount of heat locally. Thermal runaway is generally avoided by adding diluent salt. In step (2) of the present invention, when metallic sodium and potassium fluorotantalate are in contact and react, due to the use of pre-heated metallic sodium, the instantaneous temperature of the reaction point is increased, and the growth of tantalum powder at the moment of reduction is affected by the temperature of the reaction point, which promotes sintering between particles and thickens the internal sintering diameter of tantalum powder. However, due to the control of other process conditions (for example, potassium fluorotantalate reacts at a low concentration), the specific surface area of tantalum powder is still well controlled, and it is easier to construct a spatial structure suitable for capacitor production between tantalum powder particles.
[0031] The melting point of sodium is 97.78 degrees. Even if solid sodium is added, it will melt into liquid quickly in the furnace. Therefore, the prior art pays little attention to the temperature of the metal sodium itself, but only focuses on the sodium injection temperature (that is, the temperature of the reduction container or furnace when sodium is added). Although some people may have studied the effect of increasing the sodium injection temperature, this means that the temperature in the furnace needs to be increased as a whole, which brings a greater heat load to the materials made of the reduction container and the furnace, which is not conducive to its service life. Moreover, increasing the temperature in the furnace also means greater energy consumption. The prior art may also improve its fluidity by increasing the temperature of the liquid metal sodium itself, but since the fluidity of the liquid sodium almost tends to be stable as the temperature increases to above 120°C, the metal sodium with a temperature of about 120°C or less is generally added. The inventor unexpectedly found through a large amount of research that by further increasing the temperature of the liquid metal sodium, not only the good fluidity of the liquid sodium is maintained, but also the temperature of the reduction reaction point is accurately increased without increasing the power of the heating furnace, the morphology of the tantalum powder is improved, and finally the specific volume and breakdown voltage of the tantalum powder are increased.
[0032] The tantalum powder obtained according to the present invention is subjected to high-temperature and high-vacuum heat treatment according to the prior art (or first subjected to molten salt-assisted sintering according to the invention of patent CN114210973B and then subjected to high-temperature and high-vacuum heat treatment), oxygen reduction, and acid pickling treatment, so that the tantalum powder obtained still has a high specific capacitance at a high enabling voltage, and the comprehensive electrical properties are improved, and is suitable for preparing tantalum powder for high-voltage and high-reliability capacitors. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The following drawings are provided for a better understanding of the present invention. These drawings are exemplary and are not intended to limit the scope of the present invention.
[0034] Figure 1 The scanning electron microscope picture of the tantalum powder obtained according to the present invention is given.
[0035] The figure illustrates that the obtained tantalum powder has a more uniform particle size, smoother particles, and a coarser sintering neck. DETAILED DESCRIPTION
[0036] In order to further illustrate the present invention, the preferred embodiments of the present invention are described below in conjunction with the examples, and it can be clearly seen that the objects, features and advantages of the present invention. However, these descriptions are only for further illustrating the features and advantages of the present invention, rather than for limiting the present invention. If the specific conditions are not specified in the examples, they are carried out under normal conditions. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0037] For the purpose of this specification, all numbers indicating the amount of ingredients, reaction conditions, etc. in the specification and claims should be understood as being modified by the term "about" in all cases, unless otherwise specified. Accordingly, the numerical parameters given in the following specification and the appended claims are approximate values, which may vary according to the desired properties that the present invention attempts to obtain, unless otherwise indicated. At least, and without intending to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter should be interpreted at least in accordance with the number of reported significant figures and in accordance with conventional rounding techniques.
[0038] The analysis of impurity content in tantalum powder is carried out in accordance with the Chinese standard GB / T15076.1~15076.15, and the physical properties are carried out in accordance with the provisions of the industry standard YS / T573-2015. The test of electrical properties in tantalum powder is carried out in accordance with the provisions of the Chinese standard GB / T3137.
[0039] Example
[0040] In order to further illustrate the present invention, the preferred embodiments of the present invention are described below in conjunction with the examples, and it can be clearly seen that the objects, features and advantages of the present invention. However, these descriptions are only for further illustrating the features and advantages of the present invention, rather than for limiting the present invention. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0041] For the purpose of this specification, all numbers indicating the amount of ingredients, reaction conditions, etc. in the specification and claims should be understood as being modified by the term "about" in all cases, unless otherwise specified. Accordingly, the numerical parameters given in the following specification and the appended claims are approximate values, which may vary according to the desired properties that the present invention attempts to obtain, unless otherwise indicated. At least, and without intending to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter should be interpreted at least in accordance with the number of reported significant figures and in accordance with conventional rounding techniques.
[0042] The analysis of impurity content in tantalum powder is carried out according to the Chinese standard GB / T15076.1~15076.15, and the physical properties are carried out according to the provisions of the industry standard YS / T573-2007. The leakage current and capacitance of tantalum powder are tested according to the provisions of the Chinese standard GB / T3137.
[0043] Example 1
[0044] Potassium tantalate, NaCl as a diluent, and metallic sodium are provided as raw materials. The metallic sodium is preheated to a high temperature of 180° C. for use.
[0045] Take 100kg of sodium chloride (NaCl) and put it into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Pass argon at a flow rate of 40 liters / minute. Heat it to 920℃ and start stirring. Keep it warm for 30 minutes. Then add 15kg of potassium fluorotantalate. After the temperature rises to 920℃, add 3.95kg of sodium metal at 180℃ for reduction; repeat the addition of potassium fluorotantalate and heating reduction 7 times. After adding potassium fluorotantalate for the 8th time, add 8.20kg of sodium metal for reduction. After the reduction is completed, keep it warm at 920℃ for 180 minutes under the condition of argon circulation to age the tantalum powder. Then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool it to room temperature. The mixture is taken out from the reduction container, and some by-products that do not cover the tantalum powder are separated and removed. The by-products are further separated by water acid washing, washed, purified and dried to obtain high-purity tantalum powder.
[0046] Then, the tantalum powder was doped with 50 ppm P and heated at 1450 °C and below 5.0 × 10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature, and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements, the final tantalum powder obtained was made into an anode block, energized under 150V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements. In the specific capacitance test, after the 30% H2SO4 solution test, the 10% H3PO4 solution test was used, and the measured results were listed in Table 1.
[0047] Comparative Example 1
[0048] Potassium fluorotantalate, NaCl as a diluent, and metallic sodium are provided as raw materials. The metallic sodium is preheated to 130° C. for use.
[0049] Take 100kg of sodium chloride (NaCl) and put it into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Pass argon gas at a flow rate of 40 liters / minute. Heat it to 920℃ and start stirring. Keep it warm for 30 minutes. Then add 15kg of potassium fluorotantalate. After the temperature rises to 920℃, add 3.95kg of sodium metal at 130℃ for reduction; repeat the addition of potassium fluorotantalate and heating reduction 7 times. After adding potassium fluorotantalate for the 8th time, add 8.20kg of sodium metal at 130℃ for reduction. After the reduction is completed, keep it warm at 920℃ for 180 minutes under the condition of argon circulation to age the tantalum powder. Then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool it to room temperature. The mixture is taken out from the reduction container, and some by-products that do not cover the tantalum powder are separated and removed. The by-products are further separated by water acid washing, washed, purified and dried to obtain high-purity tantalum powder.
[0050] Then, the tantalum powder was doped with 50 ppm P and heated at 1450 °C and below 5.0 × 10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature, and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements, the final tantalum powder obtained was made into an anode block, energized under 150V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements. In the specific capacitance test, after the 30% H2SO4 solution test, the 10% H3PO4 solution test was used, and the measured results were listed in Table 1.
[0051] Example 2
[0052] Potassium fluorotantalate, KCl and KF as diluents, and metallic sodium are provided as raw materials. The metallic sodium is preheated to a high temperature of 220° C. for use.
[0053] Take 50kg of potassium chloride (KCl) and 50kg of potassium fluoride (KF) and put them into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Pass argon gas at a flow rate of 60 liters / minute. Heat it to 900℃ and start stirring. Keep it warm for 30 minutes. Then add 15kg of potassium fluorotantalate. After the temperature rises to 900℃, add 4.0kg of sodium metal at 220℃ for reduction; repeat the addition of potassium fluorotantalate and heating reduction for 9 times. After adding potassium fluorotantalate for the 10th time, add 8.9kg of sodium metal at 220℃ for reduction. After the reduction is completed, keep it warm at 900℃ for 120 minutes under the condition of argon circulation to age the tantalum powder. Then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool it to room temperature. The mixture is taken out from the reduction container, and some by-products that do not cover the tantalum powder are separated and removed. The by-products are further separated by water acid washing, washed, purified and dried to obtain high-purity tantalum powder.
[0054] Then, the tantalum powder was doped with 60 ppm P and heated at 1400 °C and below 5.0 × 10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature, and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements, the final tantalum powder obtained was made into an anode block, energized under 100V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements. In the specific capacitance test, after using 30% H2SO4 solution for testing, 10% H3PO4 solution was used for testing, and the measured results are listed in Table 1.
[0055] Comparative Example 2
[0056] Potassium fluorotantalate, KCl and KF as diluents, and metallic sodium are provided as raw materials. The metallic sodium is preheated to 120° C. for use.
[0057] Take 50kg of potassium chloride (KCl) and 50kg of potassium fluoride (KF) and put them into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Pass argon gas at a flow rate of 60 liters / minute. Heat it to 900℃ and start stirring. Keep it warm for 30 minutes. Then add 15kg of potassium fluorotantalate. After the temperature rises to 900℃, add 4.0kg of 120℃ sodium metal for reduction; repeat the addition of potassium fluorotantalate and heating reduction for 9 times. After adding potassium fluorotantalate for the 10th time, add 8.90kg of 120℃ sodium metal for reduction. After the reduction is completed, keep it warm at 900℃ for 120 minutes under the condition of argon flow to age the tantalum powder. Then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool it to room temperature. The mixture is taken out from the reduction container, and some by-products that do not cover the tantalum powder are separated and removed. The by-products are further separated by water acid washing, washed, purified and dried to obtain high-purity tantalum powder.
[0058] Then, the tantalum powder was doped with 60 ppm P and heated at 1400 °C and below 5.0 × 10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature, and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements, the final tantalum powder obtained was made into an anode block, energized under 100V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements. In the specific capacitance test, after using 30% H2SO4 solution for testing, 10% H3PO4 solution was used for testing, and the measured results are listed in Table 1.
[0059] Example 3
[0060] Potassium fluorotantalate, KCl and KF as diluents, and metallic sodium are provided as raw materials. The metallic sodium is preheated to a high temperature of 180°C for use.
[0061] Take 100kg of potassium chloride (KCl) and 100kg of potassium fluoride (KF) and put them into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Pass argon gas at a flow rate of 70 liters / minute. Heat it to 900℃ and start stirring. Keep it warm for 30 minutes. Then add 10kg of potassium fluorotantalate. After the temperature rises to 920℃, add 2.50kg of 180℃ sodium metal for reduction; repeat the addition of potassium fluorotantalate and heating reduction 5 times. After adding potassium fluorotantalate for the 6th time, add 6.0kg of 180℃ sodium metal for reduction. After the reduction is completed, keep it warm at 900℃ for 120 minutes under the condition of argon circulation to age the tantalum powder. Then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool it to room temperature. The mixture is taken out from the reduction container, and some by-products that do not cover the tantalum powder are separated and removed. The by-products are further separated by water acid washing, washed, purified and dried to obtain high-purity tantalum powder.
[0062] Then, the tantalum powder was doped with 100 ppm of P and heated at 1230 °C and below 5.0 × 10 -3 Pa pressure for 1.0 hour, and then deoxidize and pickle to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature, sintering time specified in Table 1, and other conditions according to the aforementioned GB / T3137 requirements, the final tantalum powder obtained is made into an anode block, energized under 60V conditions, and then the electrical properties are tested according to the aforementioned GB / T3137 requirements. In the specific capacitance test, after using 30% H2SO4 solution for testing, 10% H3PO4 solution is used for testing, and the measured results are listed in Table 1.
[0063] Comparative Example 3
[0064] Potassium fluorotantalate, KCl and KF as diluents, and metallic sodium are provided as raw materials. The metallic sodium is preheated to a high temperature of 120° C. for use.
[0065] Take 100kg of potassium chloride (KCl) and 100kg of potassium fluoride (KF) and put them into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Pass argon gas at a flow rate of 70 liters / minute. Heat it to 900℃ and start stirring. Keep it warm for 30 minutes. Then add 10kg of potassium fluorotantalate. After the temperature rises to 900℃, add 2.5kg of sodium metal preheated to 120℃ for reduction; repeat the addition of potassium fluorotantalate and heating reduction 5 times. After adding potassium fluorotantalate for the 6th time, add 6.0kg of sodium metal at 120℃ for reduction. After the reduction is completed, keep it warm at 900℃ for 120 minutes under the condition of argon circulation to age the tantalum powder. Then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool it to room temperature. The mixture is taken out from the reduction container, and some by-products that do not cover the tantalum powder are separated and removed. The by-products are further separated by water acid washing, washed, purified and dried to obtain high-purity tantalum powder.
[0066] Then, the tantalum powder was doped with 100 ppm of P and heated at 1230 °C and below 5.0 × 10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature, and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements, the final tantalum powder obtained was made into an anode block, energized under 60V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements. In the specific capacitance test, after using 30% H2SO4 solution for testing, 10% H3PO4 solution was used for testing, and the measured results are listed in Table 1.
[0067] Table 1 Analysis results of electrical properties of finished tantalum powder
[0068]
[0069]
[0070] From Table 1 we can see that:
[0071] The present invention is suitable for manufacturing tantalum powder for high-voltage and high-reliability capacitors with higher specific capacitance. Energization is performed under relatively high voltage conditions. The obtained empowered block has high specific capacitance and low residual current. In the specific capacitance test, the difference between the test results using 30% H2SO4 solution and the test results using 10% H3PO4 solution is relatively small. The breakdown voltage test shows that it has a high breakdown voltage.
Claims
1. A method for preparing tantalum powder by reducing potassium fluorotantalate with sodium, characterized in that The reduction is carried out using preheated metallic sodium as a reducing agent, preferably, the metallic sodium temperature exceeds 180°C, more preferably 200-350°C, more preferably 200-260°C, more preferably 160-190°C and / or 210-240°C.
2. A method for preparing tantalum powder by reducing potassium fluorotantalate with sodium, comprising the following steps: (1) providing a dilute salt (selected from alkali metal halides), potassium tantalate and metallic sodium as raw materials, wherein the amount of metallic sodium is in excess relative to the amount of potassium tantalate, and the metallic sodium is preheated to 180-350° C. (preferably 200-350° C., more preferably 200-260° C., more preferably 160-190° C. and / or 210-240° C.) for use, (2) placing a diluted salt into a reduction container, evacuating the container, and then introducing an inert gas such as argon, and then heating the diluted salt in the reduction container until it melts while the inert gas is kept flowing (for example, at a flow rate of 20-100 liters / minute), (3) Add part of the potassium fluorotantalate to the reduction vessel, monitor the temperature to ensure that the potassium fluorotantalate and the dilute salt are melted, and then add preheated sodium metal to reduce the part of the potassium fluorotantalate, repeating multiple times until all the potassium fluorotantalate and sodium metal raw materials are used up. (4) After the reduction is completed, the tantalum powder is aged, and (5) Then separate the tantalum powder.
3. The method according to claim 2, wherein in step (2), evacuation and argon flow are repeated multiple times, for example 2-3 times, and / or, in step (2), the diluted salt is heated to a temperature exceeding its melting point by 80°C, preferably exceeding 150°C, more preferably exceeding 200°C, and preferably kept warm, for example for 30 minutes, and the diluted salt is preferably stirred after melting.
4. The method according to claim 2 or 3, wherein in step (3), the furnace temperature is controlled to ensure that the temperature of potassium tantalate and potassium tantalate exceeds the apparent melting point, for example, exceeds the melting point by 80°C-500°C, preferably exceeds the melting point by 150°C-450°C, and preferably, the temperature is increased after each addition of potassium tantalate.
5. A method according to claim 2 or 3 or 4, wherein In steps (3) and / or (4), an inert gas such as argon is always circulated in the reduction container.
6. A method according to claim 2 or 3 or 4, wherein After step (5), the method further includes the following steps: (6) The tantalum powder is subjected to salt bath heat treatment and / or agglomeration heat treatment, the metal magnesium chips are subjected to oxygen reduction treatment, and further pickling, purification and drying are performed to obtain a tantalum powder product.
7. The method according to any one of claims 2 to 6, further comprising doping the tantalum powder with N, P and / or B elements after step (5) and / or (6).
8. A method according to any one of claims 2 to 7, wherein In step (5), the reduction container is maintained at a positive pressure.
9. Tantalum powder produced by the production method according to any one of claims 2 to 8.
10. Use of the tantalum powder according to claim 1 or the tantalum powder according to claim 9 in capacitors.
Citation Information
Patent Citations
Preparation method of coralline high-purity tantalum powder
CN110315088A
Method for producing high surface area, low metal impurity tantalum powder
JP1993508686A
Tantalum powder producing method
RU2242329C2
Tantalum powder and process for preparing the same, and sintered anode prepared from the tantalum powder
US20170226616A1
Process for producing tantalum and columbium powder
US4149876A