Glass roll, method for producing same, and method for producing composite material
By adjusting the diameter and number of glass fiber filaments and using twill winding and drying processes, the poor productivity and poor shape of the single glass filaments formed in the prior art are solved, and high efficiency and low cost are achieved glass winding body manufacturing and composite material preparation.
Patent Information
- Application Number
- CN202380030255.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-11-22
- Filing Date
- 2023-07-20
- Publication Date
- 2024-11-12
AI Technical Summary
The existing glass winding body manufacturing method is difficult to produce a thicker and thicker glass winding body formed of a single glass raw silk, and there are problems such as poor productivity, high manufacturing cost, poor shape and difficult to relieve the glass raw silk.
By winding a single glass raw silk with the rotation axis as the center, adjusting the diameter and number of the glass fiber filaments, setting the appropriate number of windings and regression numbers, and using the twill winding and drying process to form an optimized glass winding body.
The productivity and operability of the glass winding body are improved, the shape stability and the easy-to-release and comfort of the glass raw silk are ensured, and the manufacturing cost is reduced.
Smart Images

Figure CN118946532A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a glass roll formed by winding a single glass strand around a rotation axis, a method for producing the glass roll, and a method for producing a composite material using the glass roll. Background Art
[0002] It is known that direct glass roving (DR) is a glass winding body formed by directly winding glass strands, and glass strands are a bundle of multiple glass filaments. The glass strands drawn from direct glass roving can be easily formed into a composite material with a resin by a drawing molding method, a filament winding method, etc., and are therefore widely used as reinforcing fibers for resins.
[0003] In the method for producing a glass roll, for example, molten glass is pulled out by a spinning device, and a sizing agent is applied to the surfaces of the pulled out hundreds to thousands of glass fibers by a coating device to bundle the glass fibers to form glass strands. Next, the obtained bundle is wound on a rotating winding core (coil) in a twill pattern, dried, and coated to produce a glass roll (for example, Patent Document 1).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-100904 Summary of the invention
[0007] Technical problem to be solved by the invention
[0008] As a glass winding body, there is a known roving formed by plying a plurality of glass strands. However, compared with a glass winding body (single-end roving) formed by a single glass strand, the roving requires a plying process, has poor productivity, and tends to have a high manufacturing cost. Therefore, considering the above-mentioned productivity and manufacturing cost issues, a glass winding body formed by a single glass strand and having a thicker glass strand is required.
[0009] However, when manufacturing a glass roll with a relatively thick glass strand, it is difficult to roll it into a desired shape such as a square end cheese shape. In addition, the obtained glass roll is prone to shape distortion. There is also a problem that when the glass strand is released from the obtained glass roll, it is difficult to unwind it from the inner layer.
[0010] The method for producing a glass wound body in Patent Document 1 does not take into account a glass wound body having a relatively thick glass strand, and therefore has a problem in that productivity and workability cannot be sufficiently improved when winding a relatively thick glass strand.
[0011] An object of the present invention is to provide a glass roll having excellent productivity and workability, a method for producing the glass roll, and a method for producing a composite material using the glass roll.
[0012] Technical solutions for solving technical problems
[0013] The glass wound body of the present invention is a glass wound body formed by winding a single glass strand around a rotating shaft. When the diameter of the glass fiber constituting the glass strand is 28 μm or less, the number of the glass strand is Xtex and the diameter of the glass fiber is Yμm, X / Y is satisfied. 2 >8, when observed from the direction of the above-mentioned rotation axis, the angle formed by the straight line connecting the above-mentioned rotation axis and the starting point of winding of the above-mentioned glass strand and the straight line connecting the above-mentioned rotation axis and the point where the above-mentioned glass strand is located after the start of winding is set as θ, the straight-line distance in which the above-mentioned glass strand moves less than once is defined as one-way travel, the number of times the above-mentioned glass strand performs the above-mentioned one-way travel during the period from the winding starting point to the first regression point where θ becomes 0° is set as T, and when the number of times the above-mentioned glass strand rotates around the above-mentioned rotation axis is set as N, 2.0≤N / T≤5.5 is satisfied, and the above-mentioned straight-line distance is the straight-line distance connecting the two ends of the above-mentioned glass winding body in the direction of the above-mentioned rotation axis.
[0014] In the present invention, when the height of the glass wound body in the rotation axis direction is H mm and the line width of the glass strand is W mm, it is preferable that H≥W×N is satisfied.
[0015] In the present invention, the diameter of the glass filaments is preferably 17 μm or more and 28 μm or less. In this case, it is more preferable to satisfy 2.0≤N / T≤4.0.
[0016] In the present invention, the glass strands preferably have a count of 3000 tex or more and 14000 tex or less. In this case, it is more preferable that 2.0≤N / T≤4.0 is satisfied.
[0017] The manufacturing method of the glass winding body of the present invention is characterized in that the manufacturing method is used to manufacture a glass winding body formed by winding a single glass strand around a rotating shaft, and the manufacturing method includes: a step of applying a sizing agent on the surface of a plurality of glass fibers to bundle the plurality of glass fibers to form a glass strand; a step of winding the glass strands while reciprocating the glass strands in the extending direction of the rotating shaft to perform twill winding to prepare a winding body; and a step of drying the sizing agent to form a coating on the surface of the glass strands, wherein when the diameter of the glass strands constituting the glass strands is within a range of 28 μm or less, the count of the glass strands is set to Xtex, and the diameter of the glass strands is set to Yμm, X / Y is satisfied. 2 >8. In the step of preparing the winding body, the glass strand is wound in a manner satisfying 2.0≤N / T≤5.5, wherein the angle formed by the straight line connecting the rotation axis and the starting point of winding of the glass strand when observed from the rotation axis direction and the straight line connecting the rotation axis and the point where the glass strand is located after the start of winding is set to θ, the straight-line distance in which the glass strand moves less than once is defined as unidirectional travel, the number of times the glass strand makes the unidirectional travel from the winding starting point to the first regression point where θ becomes 0° is set to T, the number of times the glass strand rotates around the rotation axis is set to N, and the straight-line distance is the straight-line distance connecting the two ends of the winding body in the direction of the rotation axis.
[0018] The preparation method of the composite material of the present invention is characterized in that the manufacturing method is used to manufacture the composite material of the above-mentioned glass strands and resin from the above-mentioned glass winding body, and the manufacturing method includes: a process of impregnating the above-mentioned glass strands pulled out from the above-mentioned glass winding body with resin to obtain glass strands impregnated with resin; and a process of cutting the above-mentioned glass strands impregnated with resin.
[0019] Effects of the Invention
[0020] According to the present invention, it is possible to provide a glass wound body excellent in productivity and workability, a method for producing the glass wound body, and a method for producing a composite material using the glass wound body. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic perspective view showing a glass roll according to one embodiment of the present invention.
[0022] Figure 2 This is a schematic diagram for explaining a method of winding a glass strand.
[0023] Figure 3 It is a schematic top view used to illustrate the regression number and the alignment root number.
[0024] Figure 4 It is a schematic perspective view showing a drum-shaped glass roll.
[0025] Figure 5 This is a schematic diagram for explaining a method for producing a glass roll according to one embodiment of the present invention. DETAILED DESCRIPTION
[0026] The preferred embodiments are described below. However, the following embodiments are merely examples, and the present invention is not limited to the following embodiments. In addition, in each of the drawings, the same reference numerals are sometimes used to indicate components having substantially the same functions.
[0027] [Glass roll]
[0028] Figure 1 This is a schematic perspective view showing a glass roll according to one embodiment of the present invention. Figure 1 The glass wound body 1 is formed by winding a single glass strand 2 around a rotation axis Z. In the present embodiment, a glass direct roving is formed by directly winding a single glass strand 2 .
[0029] The glass wound body 1 has a substantially cylindrical structure in which glass strands 2 are wound in layers in the radial direction. The inner circumference of the glass strands 2 is hollow. However, a core such as a bobbin may be disposed in the center of the glass wound body 1.
[0030] The glass strand 2 is formed by bundling a plurality of glass filaments. The plurality of glass filaments are bundled by applying a bundling agent on the surface.
[0031] When the diameter of the glass fiber 2 is within the range of 28 μm or less, the number of the glass fiber is Xtex, and the diameter of the glass fiber is Yμm, X / Y is satisfied. 2 >8.
[0032] By making the diameter of the glass filaments below the above upper limit, the toughness of the glass filaments can be suppressed from decreasing, and as a result, the glass strands 2 can be made less likely to break. 2 >8, the number of glass strands 2 can be increased without increasing the diameter of the glass filaments. Therefore, by satisfying X / Y within the range of 28 μm or less, 2 >8, the operability of the glass winding body 1 can be improved, and the thickness of the glass strand 2 can be increased to improve the safety during operation. 2 It is preferably 9 or more, more preferably 10 or more, and even more preferably 11 or more, and is preferably 50 or less, more preferably 30 or less, and even more preferably 25 or less.
[0033] In addition, for example, the X / Y ratio can be increased by increasing the number of glass fibers constituting the glass strand 2. 2 In addition, it is believed that when the number of glass filaments increases, the diameter of the glass filaments themselves tends to become thinner (when the number of bushing nozzles increases, the diameter of each bushing nozzle becomes smaller), so it becomes easier to handle.
[0034] The glass strand 2 is wound onto a rotating winding core (coil) to produce a glass winding body 1. When the glass strand 2 is wound, Figure 2 As shown, the glass strand 2 is reciprocated in the width direction of the collet 11 by using the traverse guide 10, and is wound while being twill wound. At this time, it is important to perform twill winding in an appropriate manner from the viewpoint of productivity and operability of the glass wound body 1. In addition, the width direction of the collet 11 is set to the Z1 direction which is the same direction as the rotation axis Z direction.
[0035] The inventors of the present invention focused on the number of windings as a parameter for appropriately performing bias winding, and found that the productivity and handleability of the glass roll 1 can be improved by appropriately adjusting the number of windings.
[0036] The winding number is determined by the ratio of the speed at which the glass strand 2 moves in the width direction (Z1 direction) of the collet 11 to the rotation speed of the collet 11. More specifically, the winding number is a value indicating how many times the collet 11 rotates during the unidirectional movement of the glass strand 2 in the width direction (Z1 direction) of the collet 11. In addition, the unidirectional movement corresponds to the rotation speed from the equivalent Figure 1 The glass roll 1 shown moves from the first end face 1a to the second end face 1b. The number of windings can be obtained by aligning the number of roots / regression number. Figure 3 Specify the number of regressions and alignment roots.
[0037] Figure 3 is a schematic top view used to illustrate the regression number and the alignment root number. In particular Figure 3 1 is a schematic top view of the glass roll 1 when viewed from the direction of the rotation axis Z1. Figure 3 The multiple double-dotted dashed lines in FIG. 1 are all circular imaginary lines centered on the rotation axis Z. Each imaginary line passes through point A, point B, point C, point D, and point E. These imaginary lines are used to indicate that the glass strand 2 is away from the rotation axis Z each time it is wound.
[0038] First, the regression coefficient is explained. The winding of the glass strand 2 is set to Figure 3 Point A is located at a position equivalent to Figure 1 The first end surface 1a is shown as a part. When the glass strand 2 is axially ( Figure 2After the glass strand 2 moves back and forth 0.5 times (one-way movement) in the Z1 direction, the glass strand 2 is located at point B. After the glass strand 2 moves back and forth 0.5 times in the axial direction, the glass strand 2 is located at point C. After the glass strand 2 moves back and forth once in the axial direction, the glass strand 2 is located at point D. Then, after the third round trip, the glass strand 2 reaches point E. Point B is located at the position equivalent to Figure 1 In the portion of the second end face 1b shown, points C to E are located in the portion corresponding to the first end face 1a. When the glass roll 1 is viewed from the axial direction (rotation axis Z1 direction), the angle formed by the line connecting the shortest distance from the rotation axis Z through any position on the first end face 1a to the outer periphery 3 and the line connecting the shortest distance from the rotation axis Z through another point on the first end face 1a or the second end face 1b to the outer periphery 3 is θ. For example, Figure 3 In the embodiment, the angle formed by the line F extending from the rotation axis Z through point A to the outer periphery 3 and the line G extending from the rotation axis Z through point B to the outer periphery 3 is set to θ. On the other hand, the angle θ formed by the line F extending from the rotation axis Z through point A to the outer periphery 3 and the line extending from the rotation axis Z through point E to the outer periphery 3 is 0°. The number of unidirectional advances during the period from the start of winding from point A to the return to point E where the angle θ becomes 0° is 6 times. Point E, where θ becomes 0°, is set as the return point.
[0039] The regression number is the number of one-way travels from the winding starting point of the glass strand 2 to the first regression point where the angle θ becomes 0°. In addition, when the winding of the glass strand 2 does not start from the first end face 1a, the time when the glass strand 2 first reaches the first end face 1a is set as the winding starting point of the glass strand 2. Figure 3 In the illustrated case, the regression number is 6. Alternatively, the regression point may be located at a portion corresponding to the second end surface 1b. In this case, the regression number is an odd number.
[0040] In addition, the winding of the glass strand 2 is performed under certain conditions. That is, when winding the glass strand 2, the speed at which the glass strand 2 moves in the Z1 direction and the rotation speed of the barrel clamp 11 are fixed. Therefore, when an arbitrary point of the glass strand 2 located on the first end face 1a of the glass winding body 1 is set as the first point, the number of unidirectional movements during the period from the first point as the starting point to the first return to the point where the angle θ becomes 0° is also the same as the return number. More specifically, a point located on the first end face 1a or the second end face 1b is set as the second point, and the second point is set as the first return point. That is, the angle θ formed by the line connecting the shortest distance from the rotation axis Z through the first point to the outer periphery 3 and the line connecting the shortest distance from the rotation axis Z through the second point to the outer periphery 3 when viewed from the axial direction is set to 0°. Figure 3 In the illustrated case, in the manufactured glass roll 1, the number of unidirectional travels and the number of regressions from the first point to the second point are both 6 times.
[0041] Next, the number of aligned strands is described. The number of aligned strands indicates the number of times the glass strand 2 rotates around the rotation axis Z from the winding starting point of the glass strand 2 to the first return point where the angle θ becomes 0°. In addition, when the winding of the glass strand 2 does not start from the first end face 1a, the time when the glass strand 2 first reaches the first end face 1a is set as the winding starting point of the glass strand 2. In addition, one rotation indicates that the glass strand 2 rotates 360° around the rotation axis Z.
[0042] As described above, the regression number is the number of one-way travels from the winding start point of the glass strand 2 to the first regression point where the angle θ becomes 0°.
[0043] The number of aligned strands is the number of times the glass strand 2 rotates around the rotation axis Z from the winding start point of the glass strand 2 to the first return point where the angle θ becomes 0°.
[0044] The winding number can be obtained by N / T (number of aligned roots / regression number).
[0045] In the present embodiment, by setting the number of windings to 2.0≤N / T≤5.5, it is possible to appropriately perform bias winding, and the productivity and handleability of the glass wound body 1 can be improved.
[0046] Specifically, by setting the winding number to 2.0≤N / T≤5.5, it is possible to wind into a desired shape such as a square-end cheese shape. Furthermore, when the glass wound body 1 is dried, even if the water contained in the glass wound body 1 evaporates, the glass wound body 1 is unlikely to be deformed. Furthermore, when the glass strands 2 are unwound from the glass wound body 1, they can be easily unwound from the inner layer, and kinks can be reduced. Furthermore, the diffusion width when a predetermined external force is applied to the glass strands 2 can be made almost constant.
[0047] The regression number T is, for example, 10 to 23, preferably 11 to 19, more preferably 13 to 17. The number of aligned roots N is, for example, 20 to 110, preferably 30 to 90, more preferably 50 to 70.
[0048] In the present invention, when the glass strand 2 is thick, the number of windings is preferably 2.0≤N / T≤4.5, more preferably 2.0≤N / T≤4.0, further preferably 2.0≤N / T≤3.5, and particularly preferably 2.0≤N / T≤2.5. In this case, the productivity and handling properties of the glass wound body 1 can be further improved.
[0049] On the other hand, when the thickness of the glass strand 2 is relatively thin, the number of windings is preferably 3.0≤N / T≤5.5, more preferably 3.5≤N / T≤5.5, further preferably 4.0≤N / T≤5.5, particularly preferably 4.5≤N / T≤5.5, and most preferably 5.0≤N / T≤5.5. In this case, the productivity and handling properties of the glass wound body 1 can be further improved.
[0050] When manufacturing the glass roll 1, as the winding speed (spinning speed) of the molten glass decreases, the thickness of the glass strands 2 increases. On the other hand, as the winding speed (spinning speed) of the molten glass increases, the thickness of the glass strands 2 decreases.
[0051] In the case where the glass strand 2 is thick and the winding speed is low, if the number of windings is too large, it is difficult to generate appropriate tension on the glass strand 2, and a loosely wound glass roll 1 is likely to be obtained. In this case, when the glass roll 1 is transported, fingerprints or jig marks are likely to remain, sometimes resulting in a poor shape. Therefore, when the glass strand 2 is thick, it is preferred to set the number of windings to a low value as described above.
[0052] On the other hand, when the glass strands 2 are thin and the winding speed is high, if the number of windings is too small, excessive tension is likely to be generated on the glass strands 2, and quality defects such as a large amount of fuzz may occur on the glass strands 2 unwound from the glass wound body 1. In addition, the shape of the glass wound body 1 may become Figure 4 Therefore, when the thickness of the glass strand 2 is small, it is preferable to set the number of windings to a high value as described above.
[0053] In addition, when the thickness of the glass strand 2 is relatively thick, the count of the glass strand 2 is, for example, 4000 tex or more and 14000 tex or less, preferably 4800 tex or more and 14000 tex or less, and more preferably 9200 tex or more and 14000 tex or less. The diameter of the glass fiber constituting the glass strand 2 is, for example, 17 μm or more and 28 μm or less, preferably 20 μm or more and 28 μm or less, and more preferably 24 μm or more and 28 μm or less.
[0054] When the thickness of the glass strand 2 is relatively thin, the count of the glass strand 2 is, for example, 1200 tex or more and less than 4000 tex, preferably 1200 tex or more and 2400 tex or less. The diameter of the glass filaments constituting the glass strand 2 is, for example, 10 μm or more and 17 μm or less, more preferably 12 μm or more and 17 μm or less, and further preferably 14 μm or more and 17 μm or less.
[0055] In addition, the number of glass strands 2 can be adjusted by the diameter of the glass filaments, the number of glass filaments and the composition of the glass filaments. In addition, the diameter of the glass filaments can be adjusted by, for example, changing the viscosity of the molten glass in the manufacturing method described later, the winding speed during winding, etc.
[0056] In addition, the thickness of the glass strands 2 does not substantially change before and after the sizing agent is dried. Therefore, the above-mentioned count of the glass strands 2 is applicable to both before and after the sizing agent is dried.
[0057] In the present embodiment, the height of the glass wound body 1 is the dimension along the rotation axis Z1 direction of the glass wound body 1. When the height of the glass wound body 1 is set to H mm and the line width of the glass strand 2 is set to W mm, it is preferred to satisfy H ≥ W × N. In addition, N is the number of aligned strands. When H ≥ W × N is satisfied, it is possible to further suppress the shape defects of the glass wound body 1 and the glass strand 2 from being thrown off the first end face 1a or the second end face 1b.
[0058] The height H of the glass roll 1 can be set to, for example, 80 mm to 350 mm. The inner diameter of the glass roll 1 can be set to, for example, 100 mm to 250 mm. The outer diameter of the glass roll 1 can be set to, for example, 260 mm to 300 mm.
[0059] The line width W of the glass strand 2 can be set in the range of, for example, 2.0 mm to 11.0 mm, preferably 3.5 mm to 10.5 mm, more preferably 3.5 mm to 9.0 mm, and even more preferably 4.0 mm to 5.5 mm.
[0060] As described above, in this embodiment, when the diameter of the glass filament is within the range of 28 μm or less, the number of the glass filaments 2 is Xtex, and the diameter of the glass filaments 12 is Yμm, X / Y is satisfied. 2 >8, therefore, the number of glass strands 2 can be increased without increasing the diameter of the glass filaments. Furthermore, even if the number of glass strands 2 is increased, the productivity and handling properties of the glass wound body 1 can be improved by setting the winding number (N / T) to an appropriate value.
[0061] [Method for producing glass wound body]
[0062] Below, refer to Figure 5 The method for producing the glass wound body 1 will be described.
[0063] First, form Figure 5The glass fibers 12 shown in the figure are formed into a plurality of glass fibers. More specifically, the glass raw materials put into the glass melting furnace are melted to form molten glass. After the molten glass is homogenized, the molten glass is pulled out from a heat-resistant nozzle attached to the bushing. Then, the pulled molten glass is cooled to form a plurality of glass fibers (monofilaments) 12. In addition, as the bushing, for example, a platinum bushing can be used.
[0064] The composition of the glass fiber 12 is not particularly limited, and for example, E glass, S glass, D glass, AR glass, etc. can be used. Among them, E glass is cheap and can further improve the mechanical strength of the composite material when combined with resin, so it is preferred. In addition, S glass can further improve the mechanical strength of the composite material, so it is preferred.
[0065] The number of glass filaments 12 is not particularly limited, preferably more than 2000, more preferably more than 4000, further preferably more than 4001, particularly preferably more than 4500, preferably less than 10000, more preferably less than 8000. When the number of glass filaments 12 is above the above lower limit, the thickness of the glass strand 2 can be made thicker. Moreover, the mechanical strength of the composite material can be further improved when it is composited with a resin. In addition, when the number of glass filaments 12 is below the above upper limit, the length of each glass filament 12 can be made more easily consistent.
[0066] Next, a sizing agent is applied to the surfaces of the obtained plurality of glass fibers 12 by a sizing agent application mechanism 13. In a state where the sizing agent is evenly applied, the plurality of glass fibers 12 are aligned and bundled. The plurality of glass fibers 12 are aligned and bundled, for example, by a bundling shoe 14. Thus, the glass strands 2 are formed.
[0067] The sizing agent may contain thermoplastic resins such as polypropylene resin, nylon resin, polyvinyl acetate or polyphenylene sulfide resin. In addition, the sizing agent may also contain thermosetting resins such as polyester (unsaturated polyester) resin, epoxy resin or polyurethane resin. The sizing agent may also contain components such as lubricants, nonionic surfactants or antistatic agents. The proportion of these components may be appropriately set as needed.
[0068] Next, the glass strand 2 is reciprocated in the direction of the rotation axis Z1 by the traverse guide 10 to perform twill winding, and is wound up using, for example, a collet 11 to produce a wound body 15. When winding up the glass strand 2, a collet 11 having a diameter of, for example, 100 mm to 250 mm can be used. In addition, the diameter of the collet 11 is preferably 200 mm or less, and more preferably 150 mm or less.
[0069] The winding thickness of the glass strands 2 in the wound body 15 is preferably 60 mm or more and preferably 65 mm or less. When the winding thickness of the glass strands 2 in the wound body 15 is within the above range, the glass wound body 2 can be heated and dried more uniformly from the winding start portion to the winding end portion.
[0070] Next, the sizing agent is heated and dried to evaporate the water, thereby forming a coating on the surface of the glass filaments 12. As a heating and drying method, for example, hot air drying or dielectric drying can be used. The heating and drying can be performed at a temperature range of 100° C. to 150° C. for 1 hour to 24 hours. In this way, the glass wound body 1 can be obtained.
[0071] In addition, the heating and drying is preferably hot air drying. In this case, the glass strands 2 can be heated and dried more evenly from the winding start portion to the winding end portion. When hot air drying is used, the sizing agent can be kept at a temperature within a certain range more easily and reliably, so it is preferred. In addition, hot air drying and dielectric drying can also be used together.
[0072] In the manufacturing method of the present embodiment, when winding the glass roll 1, the number of windings is set to 2.0≤N / T≤5.5. This allows appropriate diagonal winding, and improves productivity and handling properties of the glass roll 1.
[0073] The glass roll 1 produced as described above can be wound into a roll shape (roll shape), stored in this shape, and used as needed. The glass roll 1 wound into a roll shape can be stored after being wrapped with an organic film material such as shrink wrap, stretch film, etc. that matches the purpose for the purpose of dust and dirt prevention and fiber surface protection. It can also be stored in a state of stacking multiple layers.
[0074] A composite material can be made by compounding the glass strands 2 pulled out from the glass winding body 1 with a resin. The following describes a method for making a composite material by a drawing molding method. First, the glass strands 2 pulled out from the glass winding body 1 are impregnated with a resin to obtain a glass strand impregnated with the resin. Specifically, the glass strands 2 pulled out from the glass winding body 1 are impregnated with a molten resin, and then cooled to solidify the molten resin, thereby obtaining a glass strand impregnated with the resin. By cutting the obtained glass strand impregnated with the resin, a granular composite material can be obtained. By injection molding the obtained granular composite material, a glass fiber reinforced resin molded body of a desired shape can be obtained.
[0075] The present invention will be described in more detail below based on specific examples. The present invention is not limited to the following examples and can be implemented with appropriate changes without changing the gist of the present invention.
[0076] (Examples 1 to 12 and Comparative Examples 1 to 7)
[0077] First, molten glass composed of E glass is pulled out from the bushing to obtain a plurality of glass fibers. Next, a sizing agent is applied to the surface of the obtained glass fibers using an applicator in such a manner that the heat loss is 0.3% to 1% by mass, and the glass fibers are bundled to obtain glass strands. Using a traverse wire guide device, the obtained glass strands are reciprocated in the axial direction for lateral movement while being wound on a 150 mm diameter barrel clamp to form a winding body. Next, the obtained winding body is heated and dried in a hot air drying furnace at a temperature of 150°C for 720 minutes to obtain a glass winding body.
[0078] In each of the examples and comparative examples, the number of glass strands (X), the diameter of the glass strands (Y), and the ratio of X / Y 2 , the winding height (H) of the glass winding body and the line width (W) of the glass strand are shown in the following Table 1. In addition, in each embodiment and comparative example, when winding the glass strand, the alignment number (N), regression number (T) and winding number (N / T) of the glass strand are set as shown in the following Table 1.
[0079] In addition, the winding shape of the glass wound body obtained in each Example and Comparative Example was evaluated according to the following evaluation criteria. The results are shown in Table 1 below.
[0080] <Evaluation Criteria>
[0081] ○: A glass wound body having a desired square-end cheese shape can be obtained.
[0082] ×: A desired glass roll in the shape of square-end cheese could not be obtained.
[0083] [Table 1]
[0084]
[0085] As is clear from Table 1, the glass rolls of Examples 1 to 12 are excellent in productivity and workability. On the other hand, the glass rolls of Comparative Examples 1 to 4 and 6 to 7 cannot obtain the desired winding shape, and have problems in productivity and workability as described in the Remarks column. In Comparative Example 5, although the desired winding shape was obtained, there was a problem in workability as described in the Remarks column.
[0086] Description of Reference Numerals
[0087] 1: glass winding body; 1a, 1b: first end face, second end face; 2: glass strand; 3: peripheral portion; 10: traverse guide; 11: cartridge; 12: glass filament; 13: bundling agent coating mechanism; 14: bundling clamp; 15: winding body.
Claims
1. A glass winding body, characterized in that: The glass winding body is a glass winding body formed by winding a single glass strand around a rotating axis. In the range where the diameter of the glass filaments constituting the glass raw yarn is 28 μm or less, when the count of the glass raw yarn is Xtex and the diameter of the glass filament is Y μm, X / Y is satisfied. 2 >8, The angle between the straight line connecting the rotating axis and the starting point of winding of the glass strand and the straight line connecting the rotating axis and the point where the glass strand is located after winding starts is defined as θ, and the straight line distance that the glass strand moves once or less is defined as a one-way movement, which is the straight line distance connecting the two ends of the glass winding body in the direction of the rotating axis. When T is the number of times the glass strand travels in one direction while the glass strand reaches the first regression point where θ becomes 0° from the winding start point and N is the number of times the glass strand rotates around the rotation axis, 2.0≤N / T≤5.5 is satisfied.
2. The glass wound body according to claim 1, characterized in that: When the height of the glass wound body in the direction of the rotation axis is H mm and the line width of the glass strand is W mm, H≥W×N is satisfied.
3. The glass wound body according to claim 1 or 2, characterized in that: The diameter of the glass filaments is greater than or equal to 17 μm and less than or equal to 28 μm.
4. The glass wound body according to claim 1 or 2, characterized in that: The glass raw yarn has a count of 3000 tex or more and 14000 tex or less.
5. The glass wound body according to claim 3, characterized in that: Satisfies 2.0≤N / T≤4.
0.
6. The glass wound body according to claim 4, characterized in that: Satisfies 2.0≤N / T≤4.
0.
7. A method for manufacturing a glass wound body, characterized in that: The manufacturing method is used to manufacture a glass winding body formed by winding a single glass strand around a rotating axis, and the manufacturing method comprises: A process of applying a bundling agent on the surface of a plurality of glass filaments to bundle the plurality of glass filaments to form glass strands; The step of winding the glass strands while reciprocating the glass strands in the extending direction of the rotating shaft to perform twill winding to prepare a wound body; and a step of drying the sizing agent to form a coating on the surface of the glass strands, In the range where the diameter of the glass filaments constituting the glass raw yarn is 28 μm or less, when the count of the glass raw yarn is Xtex and the diameter of the glass filament is Y μm, X / Y is satisfied. 2 >8, In the step of preparing the wound body, The glass strands are wound in a manner that satisfies 2.0≤N / T≤5.5, wherein: The angle between the straight line connecting the rotating axis and the starting point of winding of the glass strand and the straight line connecting the rotating axis and the point where the glass strand is located after winding starts is defined as θ when viewed from the rotating axis direction, and the straight line distance that the glass strand moves once or less is defined as a one-way movement, which is the straight line distance connecting the two ends of the winding body in the rotating axis direction. The number of times the glass strand travels in one direction while the glass strand reaches the first return point where θ becomes 0° from the winding start point is T, and the number of times the glass strand rotates around the rotation axis is N.
8. A method for manufacturing a composite material, characterized in that: The manufacturing method is used to manufacture the composite material of the glass strand and resin from the glass wound body according to claim 1, and the manufacturing method comprises: a step of impregnating the glass strands drawn out from the glass wound body with a resin to obtain glass strands impregnated with the resin; and The step of cutting the glass strands impregnated with the resin.