Energy-ray-crosslinkable adhesive composition, crosslinked adhesive, adhesive sheet, and methods for producing energy-ray-crosslinkable adhesive composition, crosslinked adhesive, and adhesive sheet
Through the combination of (meth)acrylic resin and energy ray crosslinkable acrylic resin and energy ray irradiation technology, the problem of contamination by adhesives after adhesion is solved, and the bonding effect of high adhesion and low pollution is achieved .
Patent Information
- Application Number
- CN202380030477.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-29
- Publication Date
- 2024-11-12
AI Technical Summary
During the crosslinking reaction, existing energy-ray crosslinking adhesives are contaminated by adhesives after adhesion, and there are problems of sticking traces and blurring.
Using a composition of (meth)acrylic resin and an acrylic resin with energy ray crosslinking properties, by adjusting its proportion and structure, an energy ray crosslinking adhesive is formed, combined with melt kneading and energy ray irradiation technology. A crosslinked adhesive with good adhesion was prepared.
After pasting, the bonding effect is achieved, with less contamination by adhesives and good adhesion, avoiding the pollution problems caused by residual body of low molecular weight, and having shape following and low temperature adhesion ability.
Smart Images

Figure CN118946645A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an energy-ray crosslinkable adhesive composition, a crosslinked adhesive, and an adhesive sheet, and methods for producing the same. Background Art
[0002] PSA sheets are used in a wide range of industrial fields, such as labels for displaying various information, fixing or temporarily fixing parts in the fields of OA equipment, home appliances, automobiles, and construction, and masking.
[0003] Among them, hot melt adhesives are widely used as adhesives for PSA sheets. Hot melt adhesives can be easily applied to substrates or the like by heating and melting without using a solvent, and therefore have an excellent advantage of being able to reduce environmental burden when producing PSA sheets.
[0004] As hot melt adhesives, for example, synthetic rubber hot melt adhesives are widely known. In addition, demands for reduction of environmental burdens have increased, and in recent years, acrylic hot melt adhesives and the like have also been developed (for example, Patent Document 1).
[0005] Sometimes, cohesive force is required for adhesives not limited to hot melt adhesives, and one method for imparting cohesive force is to crosslink the adhesive by irradiation with energy rays. For example, Patent Documents 2 and 3 disclose an adhesive in which a hydrogen abstraction type photoinitiator is used to abstract hydrocarbons of an acrylic resin to generate free radicals in the acrylic resin, and a crosslinking reaction is carried out by a coupling reaction of the generated free radicals.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2021-130760
[0009] Patent Document 2: Japanese Patent Application Publication No. 2011-140576
[0010] Patent Document 3: Japanese Patent Application Publication No. 2016-169304 Summary of the invention
[0011] Problems to be solved by the invention
[0012] However, when a low molecular weight hydrogen abstraction type photoinitiator is used as in the adhesives of Patent Documents 2 and 3, low molecular weight bodies generated by the free radical coupling reaction of the photoinitiator remain during the cross-linking reaction. When the adhesive sheet is adhered to the adherend and then peeled off, there is a risk of contaminating the adherend by leaving traces (blurring, ghost) of the adhesive sheet from the low molecular weight body.
[0013] The present invention has been completed in view of the above-mentioned problems, and its subject is to provide an energy-ray cross-linkable adhesive composition that can form an adhesive having good adhesion and little contamination by adherends, an adhesive sheet using the energy-ray cross-linkable adhesive composition, a cross-linked adhesive formed by energy-ray cross-linking the energy-ray cross-linkable adhesive composition and a method for manufacturing the same, and an adhesive sheet using the cross-linked adhesive and a method for manufacturing the same.
[0014] Solutions to the problem
[0015] The present inventors have found that the above-mentioned problems can be solved by using a (meth)acrylic resin and an acrylic resin having a specific structure, thereby completing the present invention.
[0016] That is, the present invention provides the following [1] to
[11] .
[0017] [1] An energy-ray crosslinkable adhesive composition comprising:
[0018] (A) a (meth)acrylic resin which is not crosslinkable by energy rays, and
[0019] (B) Energy-ray-crosslinkable acrylic resin.
[0020] [2] The energy-ray crosslinkable adhesive composition according to [1] above, wherein
[0021] The content of the energy-beam-crosslinkable acrylic resin (B) is 5 to 90 parts by mass based on 100 parts by mass of the energy-beam-non-crosslinkable (meth)acrylic resin (A).
[0022] [3] The energy-ray-crosslinkable pressure-sensitive adhesive composition according to [1] or [2] above, wherein
[0023] The energy-ray-crosslinkable acrylic resin (B) is an acrylic resin having a benzophenone structure in a side chain.
[0024] [4] The energy-ray crosslinkable adhesive composition according to any one of [1] to [3] above, wherein
[0025] The glass transition temperature of the (A) non-energy-ray-crosslinkable (meth)acrylic resin is 0° C. or lower, and the glass transition temperature of the (B) energy-ray-crosslinkable acrylic resin is 0° C. or lower.
[0026] [5] A pressure-sensitive adhesive sheet comprising an energy-crosslinkable pressure-sensitive adhesive composition layer formed from the energy-crosslinkable pressure-sensitive adhesive composition according to any one of [1] to [4] above on a substrate or a release liner.
[0027] [6] A method for producing a pressure-sensitive adhesive sheet, which is a method for producing the pressure-sensitive adhesive sheet described in [5] above, the method comprising:
[0028] The energy-ray-crosslinkable adhesive composition is obtained by melt-kneading the (A) non-energy-ray-crosslinkable (meth) acrylic resin and the (B) energy-ray-crosslinkable acrylic resin,
[0029] The energy-ray crosslinkable adhesive composition layer is formed by melt-coating the energy-ray crosslinkable adhesive composition on the substrate or release liner.
[0030] [7] A cross-linked adhesive obtained by irradiating the energy-ray cross-linkable adhesive composition according to any one of [1] to [4] above with energy rays.
[0031] [8] A method for producing a cross-linked adhesive, which is a method for producing the cross-linked adhesive described in [7] above, the method comprising:
[0032] A step of irradiating the energy-ray crosslinkable pressure-sensitive adhesive composition with energy rays.
[0033] [9] A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer formed from the cross-linked pressure-sensitive adhesive described in [7] above on a substrate or a release liner.
[0034]
[10] A method for producing a pressure-sensitive adhesive sheet, which is a method for producing the pressure-sensitive adhesive sheet according to [9] above, the method comprising:
[0035] forming an energy-ray cross-linkable adhesive composition layer formed of the energy-ray cross-linkable adhesive composition on the substrate or release liner; and
[0036] A step of irradiating the energy ray-crosslinkable pressure-sensitive adhesive composition layer with energy rays.
[0037]
[11] The method for producing a pressure-sensitive adhesive sheet according to
[10] above, comprising:
[0038] The energy-ray-crosslinkable adhesive composition is obtained by melt-kneading the (A) non-energy-ray-crosslinkable (meth) acrylic resin and the (B) energy-ray-crosslinkable acrylic resin,
[0039] The energy-ray crosslinkable adhesive composition layer is formed by melt-coating the energy-ray crosslinkable adhesive composition on the substrate or release liner.
[0040] Effects of the Invention
[0041] According to the present invention, there can be provided an energy-ray cross-linkable adhesive composition having good adhesive strength and capable of forming an adhesive with little contamination by adherends, an adhesive sheet using the energy-ray cross-linkable adhesive composition, a cross-linked adhesive obtained by energy-ray cross-linking the energy-ray cross-linkable adhesive composition and a method for producing the same, and an adhesive sheet using the cross-linked adhesive and a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a schematic cross-sectional view showing an example of the structure of the pressure-sensitive adhesive sheet of the present invention.
[0043] Figure 2 This is a schematic cross-sectional view showing another example of the structure of the pressure-sensitive adhesive sheet of the present invention.
[0044] Figure 3 This is a schematic cross-sectional view showing another example of the structure of the pressure-sensitive adhesive sheet of the present invention.
[0045] Explanation of symbols
[0046] 1 Energy-ray crosslinkable adhesive composition layer
[0047] 2, 2a, 2b Release liner
[0048] 3 Adhesive layer
[0049] 4 Substrate
[0050] 10a, 20a, 30a First adhesive sheet
[0051] 10b, 20b, 30b Second adhesive sheet DETAILED DESCRIPTION
[0052] In this specification, regarding the preferred numerical range (e.g., content range), the lower limit and upper limit described in the segment can be independently combined. For example, according to the description of "preferably 10 to 90, more preferably 30 to 60", the "preferable lower limit (10)" and the "more preferably upper limit (60)" can be combined to "10 to 60".
[0053] In this specification, "energy ray" refers to a ray having an energy quantum in an electromagnetic wave or a charged particle beam, and examples thereof include ultraviolet rays, radiation, electron beams, etc. Ultraviolet rays can be irradiated using, for example, an electrodeless lamp, a high-pressure mercury lamp, a metal halide lamp, a UV-LED, etc. as an ultraviolet source. Electron beams can be irradiated with electron beams generated by electron beam accelerators, etc. It should be noted that, as energy rays in one embodiment of the present invention, ultraviolet rays are preferably used among the above energy rays.
[0054] In the present specification, "energy ray crosslinkability" refers to a property of forming a crosslinked structure by irradiation with energy rays.
[0055] In this specification, "(meth)acrylic acid" is used as a term representing one or both of "acrylic acid" and "methacrylic acid". Similarly, "(meth)acrylate" is used as a term representing one or both of "acrylate" and "methacrylate".
[0056] In addition, in this specification, "weight average molecular weight (Mw)" is a value measured by gel permeation chromatography (GPC) method and is converted into standard polystyrene, and specifically, it is a value measured based on the method described in Examples.
[0057] The mechanism of action described in this specification is a presumed mechanism and does not limit the mechanism by which the effects of the present invention are exerted.
[0058] [Energy beam crosslinkable adhesive composition]
[0059] An energy-ray-crosslinkable adhesive composition as one embodiment of the present invention contains (A) a (meth) acrylic resin that is not energy-ray-crosslinkable (hereinafter referred to as "(A) energy-ray non-crosslinkable (meth) acrylic resin" or simply "(A) component"), and (B) an acrylic resin that is energy-ray-crosslinkable (hereinafter referred to as "(B) energy-ray crosslinkable acrylic resin" or simply "(B) component").
[0060] The energy-ray crosslinkable adhesive composition (hereinafter also referred to as "adhesive composition") forms a crosslinked structure by irradiation with energy rays to form a crosslinked adhesive. That is, the adhesive composition is a composition that is intended to be irradiated with energy rays before or after being attached to an adherend.
[0061] The adhesive composition can be irradiated with energy rays at any time, so the adhesive composition has a high degree of freedom in its production method and use method.
[0062] Specifically, since the adhesive composition does not form a desired cross-linked structure, it can be melted by heating and is suitable as a hot melt adhesive.
[0063] In addition, since the adhesive composition does not form a desired cross-linked structure, it has excellent shape-conforming properties. Therefore, the adhesive composition can also be used for applications where it is attached to an adherend having a height difference and then irradiated with energy rays to form a cross-linked adhesive.
[0064] Next, each component contained in the above-mentioned adhesive composition will be described in detail.
[0065] <(A) Energy-ray non-crosslinkable (meth)acrylic resin>
[0066] (A) The energy ray non-crosslinkable (meth)acrylic resin is not particularly limited as long as it is a (meth)acrylic resin that is not energy ray crosslinkable.
[0067] Among these, from the viewpoint of suppressing an increase in viscosity when the pressure-sensitive adhesive composition is continuously heated at a high temperature, it is more preferred that the adhesive composition not have a radically polymerizable unsaturated double bond.
[0068] (A) The (meth)acrylic resin not having energy ray crosslinkability may be used alone or in combination of two or more.
[0069] (A) The (meth)acrylic resin not having energy-ray crosslinkability is a polymer containing an acrylic monomer as a monomer component and is not particularly limited as long as it has energy-ray crosslinkability, but preferably contains a structural unit derived from an alkyl (meth)acrylate.
[0070] As the alkyl (meth)acrylate used in the component (A), for example, alkyl (meth)acrylates having an alkyl group with 1 to 18 carbon atoms can be preferably used. Specifically, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, n-tridecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, stearyl (meth)acrylate, and the like can be mentioned.
[0071] The content of the (A) non-energy-ray-crosslinkable (meth) acrylic resin in the adhesive composition of one embodiment of the present invention may be 40 to 95% by mass, 50 to 90% by mass, or 60 to 85% by mass relative to the total amount of the adhesive composition (100% by mass).
[0072] The glass transition temperature (Tg) of the (meth)acrylic resin (A) which is not crosslinkable by energy rays is usually 0° C. or lower, preferably -20° C. or lower, and more preferably -30° C. or lower. When the glass transition temperature (Tg) is 0° C. or lower, adhesive performance is easily exhibited, when it is -20° C. or lower, sufficient adhesive strength can be obtained when pasting in a low temperature environment, and when it is -30° C. or lower, more sufficient adhesive strength can be obtained.
[0073] Here, the glass transition temperature (Tg) refers to a value measured at a heating rate of 20° C. / min using a differential scanning calorimeter in accordance with JIS K 7121:1987.
[0074] <(B) Energy-beam cross-linkable acrylic resin>
[0075] (B) The energy-beam crosslinkable acrylic resin is not particularly limited as long as it is an energy-beam crosslinkable acrylic resin.
[0076] (B) The energy-beam crosslinkable acrylic resin may be used alone or in combination of two or more.
[0077] (B) The energy-beam crosslinkable acrylic resin may be, for example, an acrylic resin having an energy-beam reactive group that reacts upon irradiation with energy beams and contributes to the formation of a crosslinked structure.
[0078] Examples of the energy ray reactive group include energy ray reactive groups that are excited by irradiation with energy rays and generate radicals that induce a crosslinking reaction.
[0079] Specific examples of the energy-ray-reactive group include functional groups having a benzophenone structure, a benzyl structure, an o-benzoylbenzoate structure, a thioxanthone structure, a 3-coumarin ketone structure, a 2-ethylanthraquinone structure, a camphorquinone structure, etc. Among them, the energy-ray-crosslinkable acrylic resin (B) preferably has a benzophenone structure in the side chain.
[0080] When (B) the energy beam crosslinkable acrylic resin has a benzophenone structure, for example, the benzophenone structure abstracts hydrogen atoms from hydrocarbon groups included in the side chains of the acrylic resin by energy beam irradiation, and the radicals are re-bonded to form a crosslinked structure.
[0081] It should be noted that, from the viewpoint of easily forming a crosslinked structure, it is preferred to introduce an energy-beam-reactive group into the side chain of the acrylic resin. That is, the (B) energy-beam-crosslinkable acrylic resin is preferably an acrylic resin having a benzophenone structure in the side chain.
[0082] The content of the energy-ray reactive group in the energy-ray crosslinkable acrylic resin (B) is preferably 0.02 to 5.0 mass %, more preferably 0.05 to 3.0 mass %, based on the total amount (100 mass %) of the energy-ray crosslinkable acrylic resin (B).
[0083] The acrylic resin is a polymer containing an acrylic monomer as a monomer component and is not particularly limited as long as it has energy ray crosslinking properties, but preferably contains a structural unit derived from an alkyl (meth)acrylate.
[0084] Examples of the alkyl (meth)acrylate used in the component (B) include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, and lauryl (meth)acrylate. Among them, alkyl (meth)acrylates having an alkyl group with 1 to 8 carbon atoms are preferred, and 2-ethylhexyl (meth)acrylate, methyl (meth)acrylate, and n-butyl (meth)acrylate are more preferred.
[0085] As a method for introducing the energy-ray reactive group in component (B), for example, it can be introduced by copolymerizing a monomer having a functional group such as a vinyl group that can react with an acrylic monomer and having the energy-ray reactive group with an acrylic monomer. Alternatively, for example, it can be introduced by reacting a compound having the energy-ray reactive group with a side chain of an acrylic resin using a known method.
[0086] From the viewpoint of adhesiveness, the content of the component (B) in the above-mentioned adhesive composition is preferably 5 to 90 parts by mass, more preferably 10 to 80 parts by mass, further preferably 15 to 50 parts by mass, and further preferably 15 to 30 parts by mass, relative to 100 parts by mass of the above-mentioned component (A).
[0087] In addition, from the viewpoint of making it easier to exert the effects of the present invention, the total content of the above-mentioned (A) component and the above-mentioned (B) component is preferably 60 mass% or more, more preferably 75 mass% or more, further preferably 90 mass% or more, and is 100 mass% or less in the total amount 100 mass% of the above-mentioned adhesive composition.
[0088] The glass transition temperature (Tg) of the energy-beam crosslinkable acrylic resin (B) is preferably 0° C. or lower, more preferably -20° C. or lower, and further preferably -30° C. or lower. When the glass transition temperature (Tg) is within this range, sufficient adhesive strength can be obtained even when laminating in a low-temperature environment.
[0089] Here, the glass transition temperature (Tg) refers to a value measured at a heating rate of 20° C. / min using a differential scanning calorimeter in accordance with JIS K 7121:1987.
[0090] <Other ingredients>
[0091] The pressure-sensitive adhesive composition may or may not contain components other than the above-mentioned components.
[0092] As other components, a tackifier, a softener, an antioxidant, and adhesive additives used for general adhesives etc. are mentioned, for example.
[0093] The above-mentioned other components may be used alone or in combination of two or more.
[0094] It should be noted that in the present invention, the adhesive composition does not contain (C) a low molecular weight (Mw: 1000 or less) hydrogen abstraction type photoinitiator. In the case of containing the above-mentioned (C) component, when the above-mentioned low molecular weight hydrogen abstraction type photoinitiator crosslinks the above-mentioned (A) components, the above-mentioned (B) components, or the above-mentioned (A) component and the above-mentioned (B) component, a low molecular weight body that causes contamination of the adherend is generated as a side reaction product due to the free radical coupling reaction of the above-mentioned (C) component.
[0095] Examples of low molecular weight hydrogen abstraction type photoinitiators include aromatic ketones such as acetophenone, benzophenone, P,P'-dimethoxybenzophenone, 4-methylbenzophenone, P,P'-dichlorobenzophenone, P,P'-dimethylbenzophenone, and naphthyl acetonide. In addition, aromatic aldehydes such as terephthalaldehyde and quinone aromatic compounds such as methyl anthraquinone can also be mentioned.
[0096] The tackifier is not particularly limited, and a conventionally known tackifier can be used. Examples thereof include rosin-based resins, terpene-based resins, petroleum resins, and styrene-based resins.
[0097] The antioxidant is not particularly limited, and a conventionally known antioxidant can be used. Examples of the antioxidant include hindered phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants.
[0098] Examples of adhesive additives used in the above-mentioned general adhesives include waxes, fillers, extenders, heat stabilizers, light stabilizers, ultraviolet absorbers, colorants (pigments, dyes, etc.), flame retardants, antistatic agents, stringing inhibitors, anti-aging agents, inorganic particles, organic particles, lightweight agents, etc.
[0099] These adhesive additives may be used alone or in combination of two or more.
[0100] When these adhesive additives are contained, the content of each adhesive additive is independently preferably 0.0001 to 20 parts by mass, more preferably 0.0001 to 10 parts by mass, based on 100 parts by mass of the total of (A) the energy ray non-crosslinkable (meth) acrylic resin and (B) the energy ray crosslinkable acrylic resin.
[0101] In addition, when the above-mentioned adhesive composition contains one or more selected from the above-mentioned other components in addition to the above-mentioned (A) component and (B) component, the total content of the above-mentioned (A) component and (B) component, and one or more selected from the above-mentioned other components is preferably 60 mass% or more, more preferably 70 mass% or more, further preferably 80 mass% or more, and is less than 100 mass%, in the total amount of 100 mass% of the above-mentioned adhesive composition.
[0102] <Method for producing adhesive composition>
[0103] The pressure-sensitive adhesive composition can be produced, for example, by melt-kneading (A) a (meth)acrylic resin not crosslinkable with energy beams, (B) an acrylic resin crosslinkable with energy beams, and optional components as needed.
[0104] In the following description, the step of melt-kneading (A) the (meth) acrylic resin not having energy beam crosslinkability and (B) the acrylic resin having energy beam crosslinkability may be referred to as a “melt-kneading step”.
[0105] The melt-kneading step is, for example, a step of placing the components into a mixing device equipped with a heating device such as a heating kneader, and mixing the components in a melted state.
[0106] Examples of the mixing device including a heating device include a single-screw extruder, a twin-screw extruder, a roll mill, a Banbury mixer, an intermixer, and a pressure kneader.
[0107] When a mixing device capable of reducing pressure is used, the interior of the mixing device may be reduced in pressure as necessary to perform melt-kneading under reduced pressure.
[0108] The kneading temperature in the melt kneading step is not particularly limited, and any temperature condition that allows the components to be sufficiently mixed in a molten state may be appropriately selected, but is preferably 80 to 180°C, more preferably 100 to 170°C, and even more preferably 120 to 150°C.
[0109] It should be noted that, when the adhesive composition is produced by melt kneading, the adhesive composition does not need to contain a solvent, and from the viewpoint of reducing environmental burden, it is preferably substantially free of solvent, and more preferably free of solvent. Here, the adhesive composition "substantially free of solvent" means, for example, that the content of the solvent is preferably 0.5% by mass or less, and more preferably 0.1% by mass or less in 100% by mass of the total amount of the adhesive composition.
[0110] The PSA composition obtained after melt kneading can be directly applied to a substrate or a release liner by an extruder or the like while being heated and molten, and used for the production of a PSA sheet as one embodiment of the present invention described below, or can be filled into various containers or the like as desired, for example, without undergoing a molding step.
[0111] 〔Cross-linking adhesive〕
[0112] The cross-linked adhesive which is one embodiment of the present invention is a cross-linked adhesive obtained by irradiating an energy ray-crosslinkable adhesive composition which is one embodiment of the present invention with energy rays.
[0113] That is, the cross-linkable adhesive has a cross-linked structure formed by an energy-ray cross-linking reaction of the (B) energy-ray cross-linkable acrylic resin contained in the energy-ray cross-linkable adhesive composition.
[0114] The cross-linked adhesive itself also has good adhesive force and can also exert excellent adhesive force on the adherend. For example, from the viewpoint of not requiring an energy ray irradiation step after sticking to the adherend, the cross-linked adhesive may be formed by irradiating the adhesive composition with energy rays before sticking it to the adherend, and then sticking it to the adherend as a cross-linked adhesive.
[0115] The cross-linkable adhesive can be produced by irradiating the energy-ray cross-linkable adhesive composition with energy rays.
[0116] In addition, in the following description, the process of irradiating the said energy-ray crosslinkable adhesive composition with energy rays may be referred to as "energy-ray irradiation process".
[0117] [Adhesive sheet]
[0118] As one embodiment of the present invention, the following first and second pressure-sensitive adhesive sheets can be provided.
[0119] The first pressure-sensitive adhesive sheet is a pressure-sensitive adhesive sheet having an energy-ray cross-linkable pressure-sensitive adhesive composition layer formed from the above-mentioned energy-ray cross-linkable pressure-sensitive adhesive composition on a substrate or a release liner.
[0120] In the following description, the “energy-ray cross-linkable adhesive composition layer formed of the energy-ray cross-linkable adhesive composition” of the first adhesive sheet is also simply referred to as “adhesive composition layer”.
[0121] In addition, the "adhesive layer formed of the cross-linked adhesive" of the second adhesive sheet is also simply referred to as "adhesive layer".
[0122] In addition, when simply referred to as a "pressure-sensitive adhesive sheet", it refers to both the first pressure-sensitive adhesive sheet and the second pressure-sensitive adhesive sheet.
[0123] Next, an example of the structure of the pressure-sensitive adhesive sheet which is one embodiment of the present invention will be described using the drawings, but the present invention is not limited to the following examples.
[0124] exist Figure 1 In (a), as an example of the first PSA sheet, a PSA sheet 10a is shown which has a release liner 2 on one side of a PSA composition layer 1 and a substrate 4 on the other side of the PSA composition layer 1 .
[0125] In addition, Figure 1 In (b), as an example of the second PSA sheet, a PSA sheet 10b is shown which has a release liner 2 on one side of the PSA layer 3 and a substrate 4 on the other side of the PSA layer 3 .
[0126] The pressure-sensitive adhesive sheets 10a and 10b are suitable for applications such as pasting the exposed surface of the pressure-sensitive adhesive composition layer 1 or the pressure-sensitive adhesive layer 3 to an adherend after the release liner 2 is peeled off. Examples of such applications include label applications.
[0127] When the PSA sheet to be attached to the adherend is the first PSA sheet, after being attached to the adherend, the PSA composition layer is irradiated with energy rays to form a PSA layer composed of the crosslinked PSA.
[0128] exist Figure 2 In (a), as another example of the first adhesive sheet, a double-sided adhesive sheet 20a is shown, which has an adhesive composition layer 1 on both sides of a substrate 4, a release liner 2a on the side of one adhesive composition layer 1 opposite to the substrate 4, and a release liner 2b on the side of the other adhesive composition layer 1 opposite to the substrate 4.
[0129] In addition, Figure 2 In (b), as another example of the second adhesive sheet, a double-sided adhesive sheet 20b is shown, which has adhesive layers 3 on both sides of a substrate 4, a release liner 2a on one side of one adhesive layer 3 opposite to the substrate 4, and a release liner 2b on the other side of the other adhesive layer 3 opposite to the substrate 4.
[0130] exist Figure 3 In (a), as another example of the first PSA sheet, a substrate-free PSA sheet 30a having release liners 2a and 2b on both surfaces of the PSA composition layer 1 is shown.
[0131] In addition, Figure 3 In (b), as another example of the second PSA sheet, a substrate-free PSA sheet 30b having release liners 2a and 2b on both sides of the PSA layer 3 is shown.
[0132] The adhesive sheets 20a, 20b, 30a and 30b are suitable for laminating adherends, for example, in which the release liner 2a on one side is peeled off and removed, and the exposed surface of the adhesive composition layer 1 or the adhesive layer 3 is adhered to the adherend, and then the release liner 2b is further peeled off and removed, and the exposed surface of the adhesive composition layer 1 or the adhesive layer 3 is adhered to another adherend. Such applications include, for example, fixing or temporarily fixing various components.
[0133] It should be noted that, for the adhesive sheets 30a and 30b, when the release force when the release liner 2a is peeled off from the adhesive composition layer 1 or the adhesive layer 3 is about the same as the release force when the release liner 2b is peeled off from the adhesive composition layer 1 or the adhesive layer 3, if the two release liners are pulled outward to peel, the adhesive composition layer 1 or the adhesive layer 3 may be peeled off as the two release liners are broken. From the viewpoint of suppressing such a phenomenon, it is preferred that two types of release liners designed to have different release forces are used for the two release liners 2a and 2b.
[0134] The thickness of the adhesive composition layer in the first adhesive sheet and the thickness of the adhesive layer in the second adhesive sheet are each independently preferably 5 to 100 μm, more preferably 10 to 60 μm, and even more preferably 15 to 30 μm.
[0135] When the thickness of the adhesive composition layer and the adhesive layer is 5 μm or more, the adhesive strength tends to be further improved. When the thickness of the adhesive composition layer and the adhesive layer is 100 μm or less, the handling property tends to be better.
[0136] <Base material>
[0137] Examples of the material for forming the substrate include resins, metals, and paper materials.
[0138] Examples of the resin include: polyolefin resins such as polyethylene and polypropylene; vinyl resins such as polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol copolymer; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polystyrene; acrylonitrile-butadiene-styrene copolymer; cellulose triacetate; polycarbonate; urethane resins such as polyurethane and acrylic modified polyurethane; polymethylpentene; polysulfone; polyetheretherketone; polyethersulfone; polyphenylene sulfide; polyimide resins such as polyetherimide and polyimide; polyamide resins; acrylic resins; fluorine resins, etc.
[0139] Examples of the metal include aluminum, tin, chromium, and titanium.
[0140] Examples of the paper material include thin paper, medium-quality paper, high-quality paper, impregnated paper, coated paper, art paper, sulphate paper, and glassine paper.
[0141] The material for forming the substrate may be composed of one kind or a combination of two or more kinds.
[0142] Examples of substrates formed by combining two or more forming materials include substrates formed by laminating a paper material with a thermoplastic resin such as polyethylene, and substrates formed by forming a metal film on the surface of a resin film or sheet containing a resin. It should be noted that examples of methods for forming the metal layer include: a method of vapor-depositing the above metal by a PVD method such as vacuum evaporation, sputtering, or ion plating; or a method of attaching a metal foil formed of the above metal using a general adhesive.
[0143] In order to improve the interlayer adhesion between the substrate and other laminated layers, when the substrate contains a resin, the surface of the substrate may be subjected to surface treatment such as oxidation and embossing, or primer treatment.
[0144] Depending on the purpose of the adhesive sheet, the substrate may have, for example, an easy-adhesion layer for facilitating printing; a recording layer for realizing thermal transfer recording, inkjet recording, etc.; an outer coating film or outer lamination film for protecting their surface; information areas such as magnetic recording, bar codes, micro-semiconductor elements, etc.
[0145] On the other hand, when the pressure-sensitive adhesive sheet is made into a transparent pressure-sensitive adhesive sheet, it is preferable that the base material has transparency.
[0146] As required, the substrate may contain a substrate additive. As the substrate additive, for example, ultraviolet light absorbers, light stabilizers, antioxidants, antistatic agents, slip agents, antiblocking agents, colorants, etc. can be cited. It should be noted that these substrate additives can be used alone or in combination of two or more.
[0147] The thickness of the substrate is preferably 5 to 1000 μm, more preferably 15 to 500 μm, and even more preferably 20 to 200 μm.
[0148] When the thickness of the substrate is 5 μm or more, the deformation resistance of the PSA sheet tends to be improved. On the other hand, when the thickness of the substrate is 1000 μm or less, the handling properties of the PSA sheet tends to be improved.
[0149] In addition, the "thickness of a substrate" means the thickness of the entire substrate, and when the substrate is formed of a plurality of layers, it means the total thickness of all layers constituting the substrate.
[0150] <Release liner>
[0151] As the release liner, a double-sided release liner, a single-sided release liner, or the like can be used. Examples of the release liner include a release liner obtained by coating a release agent on a substrate for the release liner.
[0152] Examples of the release liner substrate include papers such as premium paper, glassine paper, and kraft paper; plastic films such as polyester resin films such as polyethylene terephthalate resin, polybutylene terephthalate resin, and polyethylene naphthalate resin; and polyolefin resin films such as polypropylene resin and polyethylene resin.
[0153] Examples of the release agent include rubber elastomers such as silicone resins, olefin resins, isoprene resins, and butadiene resins; long-chain alkyl resins, alkyd resins, and fluorine resins.
[0154] The thickness of the release liner is not particularly limited as long as it is within a range that does not impair the effects of the present invention, but is preferably 10 to 200 μm, more preferably 20 to 180 μm, and even more preferably 30 to 150 μm.
[0155] [Method for producing the first adhesive sheet]
[0156] The method for manufacturing the above-mentioned first adhesive sheet, for example, includes: obtaining the above-mentioned adhesive composition by melt-kneading (A) (meth) acrylic resin and (B) acrylic resin having energy-ray cross-linking properties, and forming an energy-ray cross-linking adhesive composition layer by melt-coating the energy-ray cross-linking adhesive composition on a substrate or a release liner.
[0157] In the following description, the step of forming an energy-ray crosslinkable adhesive composition layer by melt-coating the energy-ray crosslinkable adhesive composition on a substrate or a release liner may be referred to as "adhesive composition layer forming step".
[0158] In the present specification, when the release liner is subjected to release treatment on one side, the term "on the release liner" means the side subjected to release treatment.
[0159] In the method for producing the first PSA sheet, the step of melt-kneading the (A) (meth) acrylic resin and the (B) energy-beam-crosslinkable acrylic resin is as described in the melt-kneading step in the method for producing the PSA composition as one embodiment of the present invention.
[0160] The adhesive composition layer forming step may be a method of directly coating the energy-ray crosslinkable adhesive composition obtained after melt kneading on a substrate or a release liner in a heated and molten state using an extruder and a T-die etc. Then, if necessary, there may be a step of cooling the adhesive composition layer.
[0161] Through the above-mentioned pressure-sensitive adhesive composition layer forming step, a pressure-sensitive adhesive composition layer can be formed on the substrate or the release liner.
[0162] The sheet having the substrate or release liner and the PSA composition layer may be used as the first PSA sheet as one embodiment of the present invention as it is, or may be subjected to other steps to obtain a desired PSA sheet configuration as required.
[0163] For example, by attaching the release-treated surface of a release liner to the exposed surface of a PSA composition layer formed on a substrate, a film such as Figure 1 Like the PSA sheet 10a shown in (a), the PSA sheet has a release liner on one side of the PSA composition layer and a substrate on the other side of the PSA composition layer.
[0164] In addition, by attaching the substrate surface of the pressure-sensitive adhesive sheet 10a to the exposed surface of the pressure-sensitive adhesive composition layer formed on the release liner, a pressure-sensitive adhesive sheet 10a can be produced. Figure 2 Like the PSA sheet 20a shown in (a), this is a double-sided PSA sheet having PSA composition layers on both sides of a substrate, and having a release liner on the side of each PSA composition layer opposite to the substrate.
[0165] In addition, by attaching the release-treated surface of another release liner to the exposed surface of the adhesive composition layer formed on the release liner, a film such as Figure 3 This is a substrate-free PSA sheet having release liners on both sides of the PSA composition layer, such as the PSA sheet 30a shown in (a).
[0166] [Method for producing the second adhesive sheet]
[0167] The method for producing the second pressure-sensitive adhesive sheet includes, for example, the steps of forming an energy-ray crosslinkable pressure-sensitive adhesive composition layer formed from the energy-ray crosslinkable pressure-sensitive adhesive composition on a substrate or a release liner; and irradiating the energy-ray crosslinkable pressure-sensitive adhesive composition layer with energy rays.
[0168] In the method for producing the second pressure-sensitive adhesive sheet, the description of the step of forming the energy-ray-crosslinkable pressure-sensitive adhesive composition layer is the same as the description of the pressure-sensitive adhesive composition layer forming step in the method for producing the first pressure-sensitive adhesive sheet.
[0169] In the step of irradiating the energy-ray-crosslinkable pressure-sensitive adhesive composition layer with energy rays in the method for producing the second pressure-sensitive adhesive sheet, the timing of irradiating the energy rays is not particularly limited and can be appropriately determined in consideration of the method for producing the pressure-sensitive adhesive sheet, desired physical properties, and the like.
[0170] For example, the adhesive composition layer may be irradiated with energy rays directly or through a substrate or a release liner in a state where one side of the adhesive composition layer is exposed, or the adhesive composition layer may be irradiated with energy rays through a substrate or a release liner in a state where a substrate or a release liner is provided on one side and a release liner is provided on the other side.
[0171] In addition, the energy ray irradiation can be performed once or divided into multiple times. In the case of dividing into multiple times to perform the energy ray irradiation, for example, the first energy ray irradiation can be performed in a state where one side of the adhesive composition layer is exposed, and then, after a substrate or a release liner is pasted on the side, the second energy ray irradiation is performed across the substrate or the release liner.
[0172] Furthermore, the first energy ray irradiation may be performed at any time before the adhesive is attached to the adherend, and the second energy ray irradiation may be performed after the adhesive is attached to the adherend.
[0173] [Application of energy-ray crosslinkable adhesive composition, crosslinked adhesive, and adhesive sheet]
[0174] The energy-ray-crosslinkable pressure-sensitive adhesive composition, the crosslinkable pressure-sensitive adhesive, and the pressure-sensitive adhesive sheet described above as one embodiment of the present invention can be used for various purposes.
[0175] Specifically, for example, the use can be for labels, for fixing or temporarily fixing various parts, for surface protection, for sealing materials, for decoration, for display, and the like.
[0176] Among them, the use for labels and the use for fixing or temporarily fixing various parts is preferred.
[0177] The adhesive sheet for label use can be directly attached to various products, or attached to packaging films, packaging containers, etc. of various products. Examples of the constituent materials of packaging films and packaging containers include: olefin resins such as polypropylene and polyethylene; polyester resins such as polyethylene terephthalate (PET) and polylactic acid; glass, paper, metal, etc.
[0178] Among them, the pressure-sensitive adhesive sheet as one embodiment of the present invention is less likely to leave dirt on the adherend after peeling, and is therefore suitable for use in a manner of sticking to glass, metal, various products made of polyester resins, packaging containers, and the like.
[0179] The pressure-sensitive adhesive sheet for fixing or temporarily fixing is suitable for fixing or temporarily fixing electronic components, optical components, automobile parts, mechanical components, building components, decorative components, and the like.
[0180] Example
[0181] The present invention will be specifically described by the following examples, but the present invention is not limited to the following examples. It should be noted that the physical property values in each example are values measured by the following methods.
[0182] [Weight average molecular weight (Mw)]
[0183] The weight average molecular weight (Mw) was measured using a gel permeation chromatography apparatus under the following conditions and determined in terms of standard polystyrene.
[0184] (Measurement equipment)
[0185] · Measurement device: Product name "HLC-8320GPC", manufactured by Tosoh Corporation
[0186] Detector: Differential refractometer
[0187] Column: One "TSK guard column super HH", two "TSK gel super HM-H" were connected in series, and one "TSK gel super H2000" (all manufactured by Tosoh Corporation) were connected in order from the inlet side of the measurement sample.
[0188] (Measurement conditions)
[0189] Column temperature: 40℃
[0190] Elution solvent: tetrahydrofuran
[0191] Flow rate: 1.0mL / min
[0192] [Glass transition temperature (Tg)]
[0193] The glass transition temperature (Tg) is measured using a differential scanning calorimeter in accordance with JIS K 7121:1987.
[0194] (Measurement of sample mass)
[0195] 10 mg
[0196] (Measurement equipment)
[0197] · Measurement device: Product name "DSC Q2000", manufactured by TA Instruments Japan
[0198] (Measurement conditions)
[0199] ·Measurement temperature range: -80℃~50℃
[0200] Heating speed: 20℃ / min
[0201] [Thickness of each layer]
[0202] The measurement was performed at 23° C. using a constant pressure thickness tester manufactured by TECLOCK (model: “PG-02J”, in accordance with standard standards: JIS K6783, Z 1702, Z 1709).
[0203] The details of the materials used in the following Examples and Comparative Examples are as follows.
[0204] <(A) Energy-ray non-crosslinkable (meth)acrylic resin>
[0205] (Meth) acrylic resin: P(BA): polybutyl acrylate, weight average molecular weight Mw: 700000
[0206] <(B) Energy-beam cross-linkable acrylic resin>
[0207] Energy-beam crosslinkable acrylic resin: an acrylic resin having a benzophenone structure in the side chain, manufactured by BASF, trade name "acResin A204UV"
[0208] <Other ingredients>
[0209] Photoinitiator: 4-methylbenzophenone (manufactured by Lambson, trade name "SpeedCure MBP")
[0210] Examples 1 to 3, Comparative Examples 1 to 2
[0211] (Production of Energy-beam Crosslinkable Adhesive Composition)
[0212] The components (A) and (B) were blended according to the composition (unit: parts by mass) shown in Table 1, and kneaded at 130° C. for 20 minutes under nitrogen purge using a heating kneader to obtain an energy-ray crosslinkable adhesive composition.
[0213] (Manufacturing of the first adhesive sheet)
[0214] The energy-ray crosslinkable adhesive composition obtained above was directly applied to a transparent polyethylene terephthalate film (thickness: 50 μm) as a substrate in a heated and molten state using a die coater, thereby obtaining a first adhesive sheet having an energy-ray crosslinkable adhesive composition layer (thickness: 20 μm) formed of the energy-ray crosslinkable adhesive composition on the substrate.
[0215] (Manufacturing of Second PSA Sheet)
[0216] The energy-beam crosslinkable pressure-sensitive adhesive composition layer of the first pressure-sensitive adhesive sheet obtained above was irradiated with a high-pressure mercury lamp (manufactured by EYE GRAPHICS) at a cumulative light intensity of 30 mJ / cm in the UV-C region. 2 The exposed surface was irradiated with ultraviolet rays under the conditions of . Thus, an adhesive layer was formed by crosslinking the energy-ray crosslinkable adhesive composition layer of the first adhesive sheet. Then, a release-treated surface of a release liner (thickness: 38 μm) was attached to the side of the adhesive layer opposite to the substrate, thereby obtaining a second adhesive sheet having a substrate, an adhesive layer and a release liner in this order.
[0217] [Evaluation method]
[0218] The second pressure-sensitive adhesive sheet obtained in each example was evaluated by the method shown below.
[0219] [Measurement of Adhesive Strength]
[0220] After peeling off the release liner from the adhesive sheets obtained in the examples and comparative examples, the exposed adhesive surface was pressed against a stainless steel plate as an adherend at room temperature (23°C) by reciprocating a roller weighing 2 kg once in accordance with JIS Z0237:2009. After pressing, the sheets were left to stand for 30 minutes in an environment of 23°C and 50% RH (relative humidity) to prepare adhesive strength measurement samples.
[0221] The adhesive strength of the adhesive test sample prepared above was measured at 23°C and 50% RH (relative humidity) using a tensile tester (manufactured by A&D Co., Ltd., product name "TESILON (registered trademark)") in accordance with JIS Z0237:2009 by a 180° peel method at a tensile speed of 300 mm / min.
[0222] [Evaluation of Contamination of Adherents]
[0223] The second PSA sheets produced in Examples and Comparative Examples were cut into 25 mm x 50 mm pieces in a 23°C, 50% RH (relative humidity) environment to prepare two test pieces. The release liner of the test piece was removed and the exposed PSA layer was attached to an adherend (stainless steel plate).
[0224] Next, the test piece attached to the adherend was left to stand for 7 days in an environment of 70°C, and then left to stand for 1 day in an environment of 23°C, 50% RH. One of the test pieces was peeled off from the adherend by hand at a speed of about 300 mm / min along a 180° direction in an environment of 23°C, 50% RH (slow-speed peeling). In addition, another piece was peeled off by hand at a speed of about 30 m / min along a 180° direction (high-speed peeling). The state of each layer of the adhesive layer of the peeled test piece was observed with the naked eye, and the contamination of the adherend was confirmed according to the following criteria.
[0225] No contamination: Delamination occurs at the interface between the adhesive layer and the adherend, no adhesive remains on the adherend, and no difference from the unadhered portion is observed.
[0226] Blurred: Delamination occurred at the interface between the adhesive layer and the adherend, and the adhered portion was confirmed to be whiter than the unadhered portion.
[0227] Cohesive failure: The adhesive layer was broken, and the adhesive layer remained on the adherend.
[0228]
[0229] According to Table 1, the PSA sheets obtained in Examples 1 to 3 had good adhesive strength, and in the adherend contamination evaluation, no adhesion marks (blurring) of the PSA sheets were produced, no cohesive failure occurred, and no adherend contamination occurred.
[0230] On the other hand, in the PSA sheet of Comparative Example 1, which used a photoinitiator instead of the energy-ray-crosslinkable acrylic resin (B), the PSA sheet had a sticking mark (blurring). In addition, in the PSA sheet of Comparative Example 2, which did not use the energy-ray-crosslinkable acrylic resin (B), cohesive failure occurred.
Claims
1. An energy-ray crosslinkable adhesive composition comprising: (A) a (meth)acrylic resin which is not crosslinkable by energy rays, and (B) Energy-ray-crosslinkable acrylic resin.
2. The energy-ray crosslinkable adhesive composition according to claim 1, in, The content of the (B) energy-ray-crosslinkable acrylic resin is 5 to 90 parts by mass based on 100 parts by mass of the (A) non-energy-ray-crosslinkable (meth) acrylic resin.
3. The energy-ray crosslinkable adhesive composition according to claim 1 or 2, in, The energy-ray-crosslinkable acrylic resin (B) is an acrylic resin having a benzophenone structure in a side chain.
4. The energy-ray crosslinkable adhesive composition according to any one of claims 1 to 3, in, The glass transition temperature of the (A) non-energy-ray-crosslinkable (meth)acrylic resin is 0° C. or lower, and the glass transition temperature of the (B) energy-ray-crosslinkable acrylic resin is 0° C. or lower. 5 . A pressure-sensitive adhesive sheet comprising an energy-crosslinkable pressure-sensitive adhesive composition layer formed from the energy-crosslinkable pressure-sensitive adhesive composition according to claim 1 on a substrate or a release liner.
6. A method for producing an adhesive sheet, which is a method for producing the adhesive sheet according to claim 5, wherein the method include: The energy-ray-crosslinkable adhesive composition is obtained by melt-kneading the (A) non-energy-ray-crosslinkable (meth) acrylic resin and the (B) energy-ray-crosslinkable acrylic resin, The energy-ray crosslinkable adhesive composition layer is formed by melt-coating the energy-ray crosslinkable adhesive composition on the substrate or the release liner. 7 . A cross-linked adhesive obtained by irradiating the energy-ray cross-linkable adhesive composition according to claim 1 with energy rays.
8. A method for producing a cross-linked adhesive, which is a method for producing the cross-linked adhesive according to claim 7, the method comprising: A step of irradiating the energy-ray crosslinkable pressure-sensitive adhesive composition with energy rays. 9 . A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer comprising the cross-linking pressure-sensitive adhesive according to claim 7 on a substrate or a release liner.
10. A method for producing an adhesive sheet, which is a method for producing the adhesive sheet according to claim 9, wherein the method include: A step of forming an energy-ray cross-linkable adhesive composition layer formed of the energy-ray cross-linkable adhesive composition on the substrate or release liner; and A step of irradiating the energy ray-crosslinkable pressure-sensitive adhesive composition layer with energy rays.
11. The method for producing a pressure-sensitive adhesive sheet according to claim 10, wherein the method include: The energy-ray-crosslinkable adhesive composition is obtained by melt-kneading the (A) non-energy-ray-crosslinkable (meth) acrylic resin and the (B) energy-ray-crosslinkable acrylic resin, The energy-ray crosslinkable adhesive composition layer is formed by melt-coating the energy-ray crosslinkable adhesive composition on the substrate or the release liner.
Citation Information
Patent Citations
Pressure-sensitive adhesive composition, pressure-sensitive adhesive and pressure-sensitive adhesive sheet
JP2011140576A
Adhesive sheet
JP2016169304A
Hot melt adhesive composition and adhesive sheet
JP2021130760A