Method for preparing makeup-holding synthetic mica powder
Through technologies such as rinsing, desorption and purification, grinding, centrifugal sorting, spray drying and condensation modification, the problems of high surface energy and strong hydrophilicity of synthetic mica powder are solved, and small particle size, high purity and hydrophobic maintenance are prepared. Makeup synthetic mica powder, used in cosmetics, improves the dispersibility and skin feel of the product and reduces production costs.
Patent Information
- Application Number
- CN202411019175.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Traditional synthetic mica powder is difficult to disperse evenly in cosmetics due to its high surface energy, strong hydrophilicity, and easy to agglomerate, which affects the spreading ability and hiding ability of the coating, and may cause adverse reactions such as dehydration, drying, and peeling.
Through rinsing, desorption and purification, grinding, centrifugal sorting, spray drying, condensation modification and airflow dispersion, makeup-holding synthesis with small particle size, high purity, low surface energy, hydrophobic, oleophobic and anti-ultraviolet rays, it is prepared. Mica powder, modifier forms Si-O-Si binding bonds with the surface of mica powder, reducing surface energy and enhancing hydrophobicity.
The obtained makeup-holding synthetic mica powder has excellent dispersion and skin feel, and is suitable for cosmetics, which improves the makeup-holding and safety of the application, reduces production costs, and is simple and easy to scale.
Smart Images

Figure CN118948636A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to synthetic mica production and processing technology, in particular to a method for preparing long-lasting synthetic mica powder, and belongs to the technical field of synthetic mica production and processing. Background Art
[0002] Mica is a natural mineral with a unique layered structure and physical and chemical properties. It is widely used in various fields, such as electronics, coatings, plastics, rubber, cosmetics, etc. Among them, mica powder is an ideal powder raw material for making powder cosmetics because of its flaky structure, insoluble in acid, alkali, and organic solvents, and excellent adhesion to the skin. However, traditional natural mica has problems such as high heavy metal content, possible doping with carcinogen asbestos, and dark color. Therefore, synthetic mica has gradually become a new choice to replace natural mica.
[0003] The presence of hydroxyl groups (-OH) on the surface of synthetic mica powder (i.e., fluorophlogopite powder) gives it a hydrophilic surface property, and the presence of hydroxyl groups results in hydrogen bonding between synthetic mica powders, which is manifested as the smaller the particle size of the synthetic mica powder, the larger the specific surface area, and the stronger the hydrogen bonding, which ultimately leads to the synthetic mica powder being easily agglomerated into harder particles. This property is not conducive to the application of cosmetics and will produce a rough skin feel. In addition, cosmetics are generally a mixture with oil as the main dispersion system, and the hydrophilic surface of synthetic mica powder cannot be fully wetted by oil, making it difficult to disperse evenly in cosmetics, resulting in reduced spreadability and covering power of the coating, and a worse skin feel. Generally, after applying cosmetics to the skin, it is necessary to maintain a certain degree of durability under daily activity conditions, which is generally manifested as not being easily infiltrated by water, sweat, and sebum, resulting in changes in makeup. On the other hand, synthetic mica powder is usually weakly alkaline due to the presence of hydroxyl groups on the surface, and is easily prone to adverse reactions such as dehydration, dryness, and peeling after being applied to the skin surface. The suitable pH value for healthy skin is between pH 4 and 6. The weakly acidic condition can resist allergens and keep the skin healthy.
[0004] In the prior art, synthetic mica powders are usually obtained by wet grinding, and their particle size is generally 10 to 15 μm, while the particle size of mica powders required for cosmetics is usually below 10 μm, especially below 5 μm, which is also called ultrafine particle size segment. That is, it is difficult to obtain ultrafine particle size segment mica powders below 5 μm by traditional wet grinding process, mainly because it cannot solve the problem of hard agglomeration of mica powders during dehydration and drying. Although dry grinding can produce synthetic mica powders with a particle size smaller than that of wet grinding, the surface of mica is severely mechanically damaged due to the lack of liquid wetting during dry grinding, and the static electricity and additional surface energy generated by friction cannot be released. The synthetic mica powders ground by dry grinding are more likely to have hard agglomeration and frosted feeling, and cannot be used to make cosmetics. In addition, since the surface energy of synthetic mica powder itself is high, and the smaller the particle size, the higher the surface energy, the stronger the hydrophilicity, and the easier it is to agglomerate. The above technology cannot directly produce synthetic fluorphlogopite mica powders with low surface energy, hydrophobicity, and excellent dispersibility. Some researchers have coated a layer of metal oxide (usually titanium dioxide, tin oxide, silicon dioxide, etc.) on the surface of synthetic fluorophlogopite powder through liquid phase deposition reaction, and then obtained synthetic mica with low surface energy through filtering, washing, drying, calcination and dehydration. However, the process is complicated, the production cost is high and the original surface characteristics of the mica are covered. Summary of the invention
[0005] In view of the problem in the prior art that synthetic mica powder obtained by the existing method cannot be directly used in long-lasting cosmetics because it has high surface energy and hydrophilicity and is easy to agglomerate, the present invention provides a method for preparing long-lasting synthetic mica powder. According to the characteristics of the existing synthetic mica powder, the present invention obtains a long-lasting synthetic mica powder with the characteristics of small particle size, high purity, low surface energy, hydrophobicity, oleophobicity, UV resistance, skin affinity, etc. through rinsing and desorption purification, powder grinding, centrifugal separation, spray drying, condensation modification, and air flow dispersion. The long-lasting synthetic mica powder can be directly used in the production of cosmetics.
[0006] In order to achieve the above technical objectives, the technical solutions adopted by the present invention are specifically described as follows:
[0007] A method for preparing long-lasting synthetic mica powder, the method comprising the following steps:
[0008] 1) Synthetic mica flakes are dispersed in water, and then a desorbent is added and stirred. After stirring, the mixture is ground and allowed to stand for a period of time. The precipitate is then dispersed in water again, and finally a mica slurry is obtained by centrifugal separation.
[0009] 2) The mica slurry is dried by spray drying to obtain mica powder.
[0010] 3) dissolving the modifier in a solvent to obtain a modified solution, then uniformly mixing the modified solution with mica powder, then heating the mixture for reaction, and finally dispersing the mixture to obtain the long-lasting synthetic mica powder.
[0011] Preferably, the method further comprises mica pretreatment, specifically: before carrying out step 1), the synthetic mica sheets are first subjected to acid leaching treatment, and after the acid leaching is completed, the synthetic mica sheets are filtered out and washed (preferably using pure water to wash away residual acid).
[0012] Preferably, the acid is one of hydrochloric acid, sulfuric acid and nitric acid, preferably a dilute nitric acid solution with a pH value less than 1, and the acid leaching treatment time is 0.5 to 24 hours.
[0013] Preferably, in step 1), the water is pure water or deionized water, preferably pure water.
[0014] Preferably, in step 1), the mass ratio of synthetic mica powder to water is 1:5-20, preferably 1:8-15.
[0015] Preferably, in step 1), the desorbent is one or more of sodium silicate, sodium hydroxide, sodium tripolyphosphate, sodium pyrophosphate, sodium hexametaphosphate, and sodium stearate, preferably one or more of sodium hydroxide, sodium tripolyphosphate, and sodium pyrophosphate.
[0016] Preferably, in step 1), the amount of the desorbent added is 0.1-1%, preferably 0.2-0.8%, of the total mass of the synthetic mica powder.
[0017] It should be noted that in step 1), the purpose of the grinding process is to refine the mica flakes with a larger initial particle size. Any grinding technology in the prior art can be applied. Preferably, in the present invention, the grinding process is specifically: the mica flakes are ground into powder using a vertical stirred mill, and the mass ratio of mica / pure water in the grinder is controlled to be 5-10:2-3. The grinding medium in the grinder is zirconium oxide beads, and the mica flakes are ground by the relative movement and shearing action of the zirconium beads. The average particle size of the mica powder is ground to <22μm, and the upper and lower limits of the particle size are 1μm and 45μm, respectively.
[0018] Preferably, in step 1), the centrifugal separation is carried out at a feed speed of 7 to 12 m / s. 3 / h (preferably 8 to 10 m 3 / h), centrifugal differential speed of 4 to 6 (preferably 5 to 5.5), and a rotation speed of not less than 3000 r / min (preferably 3000 to 3500 r / min) to obtain mica slurry.
[0019] Preferably, in step 1), the average particle size of mica in the mica slurry is 1 to 10 μm, preferably 2 to 8 μm.
[0020] Preferably, in step 2), the spray drying is to spray the mica slurry in an atomized manner, and simultaneously blow a hot air flow along the spraying direction to evaporate and dry the mica powder so as to obtain the mica powder with a water content of less than 1 wt%.
[0021] Preferably, in step 2), the flow rate of the mica slurry spraying is 0.5-5 L / min, preferably 1-4 L / min. The hot air flow is hot air at 200-350°C, preferably hot air at 250-300°C.
[0022] Preferably, in step 3), the modifier is one or more of polymethylhydrogensiloxane, polydimethylsiloxane alcohol, hexyltrimethoxysilane, n-hexadecyltrimethoxysilane, triethoxyoctylsilane, tridecafluorooctyltriethoxysilane, retinyltrimethylsilane, and aminopropyltriethoxysilane, preferably one or more of polymethylhydrogensiloxane, polydimethylsiloxane alcohol, triethoxyoctylsilane, and tridecafluorooctyltriethoxysilane.
[0023] Preferably, in step 3), the solvent is one or more of water, ethanol, isopropanol, glycerol, and ethyl acetate, preferably one or more of pure water, ethanol, and ethyl acetate.
[0024] Preferably, in step 3), the mass concentration of the modifier in the modified solution is 1 to 30%, preferably 6 to 25%.
[0025] Preferably, in step 3), the mixing mass ratio of the modified solution to the mica powder is 1:3 to 20, preferably 1:5 to 15. The modified solution is added by spraying under stirring, wherein the addition rate of the modified solution is 2 to 5 L / min.
[0026] Preferably, in step 3), the heating reaction is carried out at 100-150° C. for 1-12 hours. Preferably, the ambient pressure of the heating reaction is negative pressure (preferably negative pressure not less than -24 KPa).
[0027] Preferably, in step 3), the dispersion treatment is performed by using a gas with a gas pressure of 0.5 to 1 MPa while a feed rate of 1 to 5 Kg / min is used.
[0028] Preferably, in step 3), a catalyst is further added to the modified solution, and the catalyst is one or more of hydrochloric acid, acetic acid, tartaric acid, citric acid, and 1,2-succinic acid, preferably one of hydrochloric acid, tartaric acid, and citric acid, and more preferably citric acid.
[0029] Preferably, in step 3), the amount of the catalyst added is 0.05-2.5% of the total mass of the modified solution, preferably 0.1-2%.
[0030] Preferably, the long-lasting synthetic mica powder has an average particle size of 1 to 10 μm, a whiteness of not less than 85, a pH of 4.5 to 6.5, a water contact angle of not less than 135°, and a product activation degree of not less than 99%.
[0031] Preferably, the structure of the long-lasting synthetic mica powder is as follows: synthetic mica is used as the core, and a modified molecular layer is coated on the surface of the synthetic mica. The hydrophobic groups of the modified molecular layer face outward, and Si-O-Si bonding bonds are formed between the inner silicon atoms and the synthetic mica. The surface bonding structure is as follows:
[0032]
[0033] Wherein, R is a hydrophobic functional group, preferably one or more of octyl, hexyl, tridecafluorooctyl, n-hexadecyl, aminopropyl, and retinyl.
[0034] In the present invention, conventional synthetic mica flakes (obtained through self-production or outsourcing) can generally be used as raw materials (the average particle size range is generally 4 to 16 meshes, and a certain degree of fluctuation can be allowed in actual production). According to its characteristics, it is subjected to targeted rinsing, desorption purification, grinding, centrifugal sorting, spray drying, condensation modification, and airflow dispersion treatments in sequence, and finally a long-lasting synthetic mica powder with an average particle size of 1 to 10 μm and high purity, low surface energy, good dispersibility, no agglomeration, hydrophobic, oleophobic, UV-resistant, and skin-friendly characteristics is obtained, which can be directly used to make cosmetics. In addition, the process of the present invention is simple and easy to operate, low in cost, and easy to mass produce.
[0035] In the present invention, the diameter distance is calculated according to the upper limit Dv(90), the lower limit Dv(10) and the median diameter Dv(50) of the mica particle size in the mica slurry obtained by centrifugal sorting as follows: diameter distance = [Dv(90) - Dv(10)] / Dv(50), as shown in the following table:
[0036] Serial number Dv(10) Dv(50) Dv(90) Diameter Mica powder 1 0.69μm 1.7μm 3.1μm 1.40 Mica powder 2 1μm 3.2μm 5.6μm 1.44 Mica powder 3 3.8μm 6.3μm 12.5μm 1.39
[0037] In the present invention, since traditional synthetic mica finished products generally contain impurities such as quartz, stevenstone, fluorite, etc., which are not conducive to the application of synthetic mica powder in cosmetics, the present invention uses water as a dispersant and a cleaning agent, that is, by separating and taking away the impurities in the synthetic mica powder. The specific method is to disperse the synthetic fluorphlogopite powder in pure water, and the ratio of water to mica powder should be as high as possible, usually 1:5~15 is more suitable. When the synthetic mica powder is put into water, it needs to be stirred at high speed, and the shear force brought by the flow velocity difference of the fluid field is used to peel off the impurities adsorbed on the surface of the mica, and dissolve in the water. After standing for a period of time, the removal of impurities is achieved through solid-liquid separation. In order to improve the impurity removal effect, a small amount of desorbent (one or more of sodium silicate, sodium hydroxide, sodium tripolyphosphate sodium pyrophosphate, sodium hexametaphosphate, sodium stearate, sodium n-dodecyl sulfate, and polyacrylamide) is also added during the process of stirring and dispersing the synthetic mica powder, and the separation effect of impurities is promoted by the addition of the desorbent, thereby improving the purity of the mica powder.
[0038] In the present invention, the soluble impurities in the mica are mainly removed by water washing and desorption, and some insoluble impurities settle together with the mica and continue to remain in the solid phase. Therefore, the present invention disperses the precipitate after rinsing, desorption and grinding in water again, and further removes the impurities by utilizing the different particle sizes and specific gravities of the impurities and the mica powder. Specifically, the centrifugal separation method is used, and the process parameters of the centrifugal separation are: at a feed speed of 7 to 12 m / s 3 / h, centrifugal differential speed of 4 to 6, and speed of not less than 3000r / min, the sorting treatment is carried out to remove the coarser particle size of the synthetic fluorphlogopite powder and impurities such as sand and gravel, so that the synthetic fluorphlogopite powder after sorting has an average particle size of 2 to 10μm. In other words, through differential centrifugal sorting, the removal of insoluble impurities is achieved, and the mica powder with relatively large particle size is also removed, so that the particle size of the mica powder is adjusted.
[0039] In the present invention, the mica is pre-treated by acid leaching before water washing and desorption, and the acid leaching can remove acid-soluble impurities adsorbed on the mica flakes, mainly acid-soluble metal oxides and fluorides such as iron oxide, ferrous oxide, magnesium fluoride, calcium fluoride, etc., thereby effectively improving the purity of the mica powder.
[0040] In the present invention, the mica slurry after centrifugal sorting has a high water content (generally greater than 80%) and is a flowing slurry material. The traditional process method is to filter, collect the filter cake and bake it to dryness, but this method is not applicable to this product, because the smaller the particle size of the mica powder, the larger the specific surface area and the higher the surface energy. The mica powder with fine particle size is very easy to agglomerate during the baking process to form large agglomerates, which makes it impossible to use it to make cosmetics. Due to the adsorption of hydroxyl (-OH) on the surface of mica, the types of agglomeration that may occur under static baking include 1) hydrogen bond agglomeration, that is, the interaction between hydroxyl groups; 2) chemical bond agglomeration, that is, the formation of -O- chemical bonds. Once this agglomeration occurs, it is almost impossible to open. Therefore, in the preparation method described in the present invention, the drying and dehydration of the synthetic fluorphlogopite powder is achieved by spray drying. The basic principle is to spray the mica powder slurry in atomization. The atomization method can be to spray with high-pressure air or to "throw out" the liquid in a mist form by centrifugal force. After atomization and spraying, the mica powder particles are dispersed in the mist, and the distance between each other can be considered infinite (compared to their particle size). At this time, hot air can be blown along the spray direction to take away the moisture within 3 to 5 seconds, achieving the purpose of drying and avoiding agglomeration. The specific process is generally: the feed liquid is sprayed in a mist at a flow rate of 0.5 to 5L / min, and hot air at 200 to 350°C is blown along the spray direction to evaporate the moisture quickly, and a cyclone separator is used to collect the dry synthetic fluorphlogopite mica powder (water content <1wt%). Deviations in process parameters will lead to insufficient drying and reduced dispersibility.
[0041] In the present invention, the basic principle of surface modification is to use chemical adsorption reaction to bond organic molecules with hydroxyl groups adsorbed on the surface of mica. The organic molecules cover the surface of mica powder with the oleophilic part facing outward. The surface-modified synthetic fluorophlogopite powder has various special properties such as oleophilicity, makeup-lasting, hydrophobicity, and UV resistance. The key to the modification treatment is the full mixing and contact between the modifier and the mica powder. Therefore, in the present invention, the modifier needs to be pretreated before the modifier contacts the mica, specifically, the modifier is fully dispersed in the solvent to form a modified solution: that is, the modifier is added to the solvent and dispersed evenly using a high-speed disperser (for example, dispersed for not less than 30 minutes at a rotation speed of 70-270r / min). By forming a uniformly dispersed solution of the modifier before use, pretreatment activation is achieved (i.e., the prepared modifier solution is fully dispersed and emulsified by high-speed stirring, and pre-reacted to form Si-OH intermediates), and then the modifier solution is added to a device containing mica powder in an atomized spray manner under high-speed stirring conditions (for example, under the condition of a rotation speed of 120 to 200 r / min, the modified solution is fed at a spray rate of 2 to 5 L / min, and after the modified solution is completely sprayed, the stirring and mixing is continued for not less than 30 minutes). That is, the present invention can achieve full mixing and dispersion of the organic modifier and the synthetic mica powder through the above process, the form of the modifier solution ensures the effectiveness of the reaction, and the process is simple.
[0042] In the present invention, the modifier is one or more of polymethylhydrogensiloxane, polydimethylsiloxane, hexyltrimethoxysilane, hexadecyltrimethoxysilane, triethoxyoctylsilane, tridecafluorooctyltriethoxysilane, retinyltrimethylsilane, and aminopropyltriethoxysilane. In particular, when tridecafluorooctyltriethoxysilane is selected as one of the modifiers, it can further reduce the surface energy of the synthetic mica powder, and it is not only hydrophobic, but also oleophobic (specifically, it exhibits hydrophobicity and oleophobicity at the same time, with a water contact angle of >135° and an oil contact angle of >100°); when retinyltrimethoxysilane is selected as one of the modifiers, since it also has a high-efficiency antioxidant, it can also improve the antioxidant property of the product, prevent the product from deteriorating, and can also play an antioxidant role when applied to cosmetics. It should be noted that when dissolving the modifier, in order to improve its solubility, it can be emulsified and dispersed by adding a surfactant, for example, the surfactant is polysorbate 80.
[0043] In the present invention, in order to further improve the modification effect, a catalyst is also added to the modification solution. Under the action of the catalyst, the uniformly dispersed modifier and mica powder are mixed and heated (generally 100-150° C.) to cause the modifier to undergo a dehydration condensation reaction with the hydroxyl groups adsorbed on the surface of the mica (the reaction time is generally 1 to 12 hours), and the reaction formula is: R1-Si(OC2H5)3+HO-Mica→R1-Si-O-Mica+3C2H5OH. In particular, negative pressure should be applied during the condensation reaction (for example, a negative pressure vacuum of not less than -24kpa), and the specific method is to use a heating oven with a sealing strip and a vacuum pump. The purpose of applying negative pressure vacuum is that since the condensation reaction is a reversible reaction, the alcohols in the reaction product are volatile, and the negative pressure vacuum can promote the volatilization of the alcohol, so that the reaction balance continues to move to the right.
[0044] In the present invention, after the dehydration condensation reaction is completed, the modified mica powder needs to be dispersed again. The specific method is to use an airflow disperser to treat the synthetic fluorphlogopite mica powder after the reaction. The airflow can open the agglomerated particles and improve the dispersibility, so that the product meets the requirements of light skin feel of cosmetics. Specific dispersion process: When the feed rate is 1 to 5 Kg / min, the gas with an airflow pressure of 0.5 to 1 Mpa is used for airflow dispersion treatment, and the target product is collected by a cyclone separator.
[0045] In the present invention, the long-lasting synthetic mica powder prepared by the method of the present invention has excellent hydrophobicity, a contact angle with water of not less than 135° (preferably above 140°), a product whiteness of not less than 85, a product pH of 4.5-6.5, and a product activation degree of 99% (the specific detection method is to place M grams of the product in pure water, stir and shake it thoroughly, and then let it stand to remove the powder floating on the water surface. The powder that has settled to the bottom is filtered out and dried, and weighed to obtain m grams; the activation index is calculated as H=(-m) / M×100%. An activation degree of >99 means that more than 99% of the powder has changed its surface properties due to the process described in the present invention). The structure of the long-lasting synthetic mica powder is specifically: synthetic mica is used as the core, and a modified molecular layer is coated on the surface of the synthetic mica. Among them, the hydrophobic group of the modified molecular layer faces outward, and Si-O-Si bonding bonds are formed between the inner silicon atoms and the synthetic mica. Its surface bonding structure is as follows:
[0046]
[0047] Wherein, R is a hydrophobic functional group, preferably one or more of octyl, hexyl, tridecafluorooctyl, n-hexadecyl, aminopropyl, and retinyl.
[0048] Compared with the prior art, the beneficial technical effects of the present invention are as follows:
[0049] 1: Based on the characteristics of traditional synthetic mica powder, the present invention adopts a special process design, specifically through rinsing and desorption purification, grinding, centrifugal separation, spray drying, condensation modification and air flow dispersion, to obtain a long-lasting synthetic mica powder with small particle size, high purity, low surface energy, hydrophobic, oleophobic, UV-resistant, skin-friendly and other characteristics, which can be directly used in the production of cosmetics.
[0050] 2: The method of the present invention has a simple process flow, low cost, and is easy to mass produce, providing a new way to high-value utilization of synthetic mica and obtain long-lasting cosmetics with better quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 This is a microscopic image of the particle size distribution of the synthetic mica powder prepared in Example 3 of the present invention.
[0052] Figure 2 This is the X-ray diffraction pattern of the synthetic mica powder prepared in Example 3 of the present invention.
[0053] Figure 3 This is a graph showing the hydrophobicity test results of the synthetic mica powder prepared in Example 3 of the present invention.
[0054] Figure 4 The following are comparison photos of the activation degree test results of the synthetic mica powder prepared in Example 3 of the present invention before and after modification.
[0055] Figure 5 The figure is an overall process flow chart of the method of the present invention. DETAILED DESCRIPTION
[0056] The technical solution of the present invention is illustrated below by way of example, and the scope of protection requested by the present invention includes but is not limited to the following embodiments.
[0057] Example 1
[0058] The synthetic mica flakes after air selection are selected and screened with a double-layer sieve. The mica flakes with a size range of 4 to 16 mesh are collected and added to a dilute nitric acid solution with a pH value less than 1 and soaked for 12 hours. The mica flakes are then filtered and washed with pure water for 3 times and then dried to obtain synthetic mica flakes.
[0059] First weigh 100kg of the above-mentioned synthetic mica flakes, put them into a rinsing kettle with an agitator, and inject 1000L of pure water. Turn on the stirring to make the mica powder completely dispersed in the water to form a slurry. Add a mixture of 0.1kg of sodium hydroxide and 0.2kg of sodium pyrophosphate to the slurry, and continue stirring for 60 minutes. After the stirring is completed, grind it again, and then let it stand for 24 hours to allow the mica powder to settle. At this time, it can be observed that the upper layer of liquid is a yellowish-brown suspension, and its turbidity is measured by a turbidity meter and is about 22NTU. Open the side drain port of the rinsing kettle and discharge the upper layer of liquid until the synthetic mica powder precipitated at the bottom is exposed. It can be observed that the color of the mica powder is shiny white. Add 850L of pure water again, continue stirring to dissolve and disperse the precipitated synthetic mica powder to form a slurry, and centrifuge the slurry: use a screw pump to feed, and maintain a flow rate of 8.5±0.5m 3 / h, adjust the centrifuge main machine speed to 3500r / min, and maintain the differential speed at 5.3±0.1; collect the suspension to obtain the target mica slurry, and detect that its average particle size is about 1.78μm.
[0060] Then, the mica slurry obtained above was injected into a spray dryer, and the feed flow rate was adjusted to 1 L / min, and the temperature of the dry hot air was adjusted to 290° C. The dried mica powder was collected, and its moisture content was measured to be about 0.82%.
[0061] Then weigh 15 kg of ethanol, 5 kg of pure water, and 0.05 kg of citric acid, mix and stir to dissolve, then add 3 kg of triethoxyoctylsilane, and pour the prepared solution into a high-speed mixer, set the stirring speed to 220 r / min, and stir for 1.5 hours to obtain a modifier solution.
[0062] Then take 100kg of spray-dried synthetic mica powder and put it into the mixing and blending machine, start the mixing and blending and set the speed to 80r / min. At this time, spray the modifier solution into the mixing and blending machine in the form of a spray, and the spray flow rate is about 2L / min. During the spraying process, gradually increase the stirring speed to 180r / min, and continue stirring for 2 hours after the modifier solution is completely sprayed. The mica powder mixed with the modifier is discharged from the mixing and blending machine, loaded into a stainless steel tray and placed in a preheated reaction vessel for condensation reaction (the ambient pressure of the reaction is controlled to be -24KPa during the reaction). The reaction temperature is set to 130°C and the reaction is carried out for 6 hours. During this period, the material needs to be loosened once every 1 hour with a stainless steel material rake. After the reaction is completed, take out the material.
[0063] The reacted materials are fed into an airflow disperser for dispersing and deagglomeration. The material feed rate is 2.5 kg / min, and the airflow pressure of the fan is adjusted to 0.7 MPa. The soft agglomerates produced during the baking process are disintegrated by high-speed airflow and collected in a cyclone separator to obtain a surface-modified synthetic fluorphlogopite powder product.
[0064] Example 2
[0065] Example 1 was repeated except that 3 kg of triethoxyoctylsilane was replaced by 3 kg of tridecafluorooctyltriethoxysilane.
[0066] Example 3
[0067] Example 1 was repeated except that 3 kg of triethoxyoctylsilane was replaced by 3 kg of polymethylhydrogensiloxane.
[0068] Example 4
[0069] Example 1 was repeated except that 3 kg of triethoxycaprylylsilane was replaced by 3 kg of dimethiconol.
[0070] Example 5
[0071] Example 1 was repeated, except that the mica flakes were immersed in a dilute nitric acid solution with a pH value less than 1 for 12 hours, and were immersed in a dilute hydrochloric acid solution with a pH value less than 3 for 6 hours.
[0072] Example 6
[0073] Example 1 was repeated, except that the mica flakes were immersed in a mixed solution of dilute hydrochloric acid and dilute sulfuric acid at pH <1 for 12 hours instead of being immersed in a dilute nitric acid solution at pH <1 for 12 hours.
[0074] Example 7
[0075] Example 1 was repeated except that 0.3 kg of the mixture of sodium hydroxide and sodium pyrophosphate was replaced by 0.3 kg of sodium silicate.
[0076] Example 8
[0077] Example 1 was repeated except that the mixture of 0.3 kg of sodium hydroxide and sodium pyrophosphate was replaced by a mixture of 0.1 kg of sodium silicate and 0.2 kg of sodium tripolyphosphate.
[0078] Example 9
[0079] Example 2 was repeated except that 0.05 kg of citric acid was replaced by 0.15 kg of acetic acid.
[0080] Example 10
[0081] Example 2 was repeated except that 0.05 kg of citric acid was replaced by 0.15 kg of citric acid.
[0082] Embodiment 11
[0083] Example 2 was repeated except that 0.05 kg of citric acid was replaced by 0.02 kg of citric acid.
[0084] Example 12
[0085] Example 10 was repeated except that 0.15 kg of citric acid was replaced by 0.15 kg of tartaric acid.
[0086] Embodiment 13
[0087] Example 4 was repeated except that 3 kg of dimethiconol was replaced by 0.1 kg of dimethiconol.
[0088] Embodiment 14
[0089] Example 4 was repeated except that 3 kg of dimethiconol was replaced by 1 kg of dimethiconol.
[0090] Embodiment 15
[0091] Example 4 was repeated except that 3 kg of dimethiconol was replaced by 2 kg of dimethiconol.
[0092] Example 16
[0093] Example 4 was repeated except that 3 kg of dimethiconol was replaced by 4 kg of dimethiconol.
[0094] Embodiment 17
[0095] Example 1 was repeated, except that the mica sheets were not treated by immersion in dilute nitric acid.
[0096] Comparative Example 1
[0097] Example 1 was repeated except that sodium hydroxide and sodium pyrophosphate were not added to the slurry.
[0098] Comparative Example 2
[0099] Example 2 was repeated except that no citric acid was added.
[0100] Comparative Example 3
[0101] Example 4 was repeated except that no dimethiconol was added.
[0102] Comparative Example 4
[0103] Example 4 was repeated except that ethanol, purified water, citric acid, triethoxyoctylsilane and 100 kg of spray-dried synthetic mica powder were put into a mixing mixer.
[0104] The following table is a comparison table of performance parameters of the products obtained from the above embodiments and comparative examples:
[0105] Whiteness Degree of activation Water contact angle Oil absorption pH Example 1 93.8 96.5 135.5° 42 / 100 5.9 Example 2 93.5 99.4 141.0° 29 / 100 6.2 Example 3 93.9 100 149.2° 26 / 100 6.0 Example 4 93.1 97.2 123.4° 40 / 100 6.1 Example 5 84.9 96.9 138.1° 43 / 100 6.3 Example 6 86.8 95.9 136.9° 45 / 100 6.2 Example 7 84.5 97.9 139.3° 39 / 100 6.2 Example 8 91.2 98.0 139.9° 38 / 100 6.1 Example 9 91.2 82.9 121.3° 58 / 100 6.8 Example 10 90.5 99.4 144.7° 28 / 100 5.5 Embodiment 11 90.8 71.2 91.5° 57 / 100 6.9 Example 12 90.8 94.2 133.1° 47 / 100 5.8 Embodiment 13 89.7 77.4 89.9° 58 / 100 6.2 Embodiment 14 88.2 86.1 128.4° 51 / 100 6.1 Embodiment 15 90.0 97.9 139.3° 39 / 100 6.2 Example 16 90.1 99.9 145.8° 27 / 100 6.2 Embodiment 17 78.3 95.5 135.8° 45 / 100 5.9 Comparative Example 1 81.6 91.1 124.7° 51 / 100 6.1 Comparative Example 2 90.9 67.6 89.9° 59 / 100 7.4 Comparative Example 3 93.6 0 0 71 / 100 7.3 Comparative Example 4 92.9 27.9 0 64 / 100 6.2
[0106] From the above table, we can know that the modification of mica with modifiers has a significant impact on the product's activation, water contact angle, pH and other parameter performances, and the use of modifiers and the different dosages will have an important impact on the results. In addition, whether a catalyst is used and the choice of catalyst during the modification process will also have a significant impact on the modification results. It should also be noted that whether the initial mica flakes are acid-leached and desorbed will not only have an important impact on the whiteness of the product, but also affect the subsequent modification effect of the mica.
Claims
1. A method for preparing long-lasting synthetic mica powder, characterized in that: The method comprises the following steps: 1) dispersing the synthetic mica flakes in water, then adding a desorbent and stirring, grinding and standing after the stirring is completed, then re-dispersing the precipitate in water, and finally centrifugally sorting to obtain mica slurry; 2) drying the mica slurry by spray drying to obtain mica powder; 3) dissolving the modifier in a solvent to obtain a modified solution, then uniformly mixing the modified solution with mica powder, then heating the mixture for reaction, and finally dispersing the mixture to obtain the long-lasting synthetic mica powder.
2. The method according to claim 1, characterized in that: The method further includes mica pretreatment, specifically: before performing step 1), the synthetic mica sheet is first subjected to acid leaching treatment, and after the acid leaching is completed, the synthetic mica sheet is filtered out and washed; Preferably, the acid is one of hydrochloric acid, sulfuric acid and nitric acid, preferably a dilute nitric acid solution with a pH value less than 1, and the acid leaching treatment time is 0.5 to 24 hours.
3. The method according to claim 1 or 2, characterized in that: In step 1), the water is pure water or deionized water, preferably pure water; preferably, the mass ratio of synthetic mica powder to water is 1:5-20, preferably 1:8-15; and / or In step 1), the desorbent is one or more of sodium silicate, sodium hydroxide, sodium tripolyphosphate, sodium pyrophosphate, sodium hexametaphosphate, and sodium stearate, preferably one or more of sodium hydroxide, sodium tripolyphosphate, and sodium pyrophosphate; preferably, the amount of the desorbent added is 0.1-1% of the total mass of the synthetic mica powder, preferably 0.2-0.8%.
4. The method according to any one of claims 1 to 3, characterized in that: In step 1), the centrifugal separation is carried out at a feed speed of 7 to 12 m / s. 3 / h (preferably 8 to 10 m 3 / h), centrifugal differential speed of 4 to 6 (preferably 5 to 5.5), and a rotation speed of not less than 3000 r / min (preferably 3000 to 3500 r / min) to obtain mica slurry; Preferably, the average particle size of mica in the mica slurry is 1 to 10 μm, preferably 2 to 8 μm.
5. The method according to any one of claims 1 to 4, characterized in that: In step 2), the spray drying is to spray the mica slurry in an atomized manner, and at the same time blow a hot air flow in the spraying direction to evaporate and dry the mica powder with a water content of less than 1wt%; Preferably, the flow rate of the mica slurry spraying is 0.5-5 L / min, preferably 1-4 L / min; the hot air flow is hot air at 200-350°C, preferably hot air at 250-300°C.
6. The method according to any one of claims 1 to 5, characterized in that: In step 3), the modifier is one or more of polymethylhydrogensiloxane, polydimethylsiloxane alcohol, hexyltrimethoxysilane, n-hexadecyltrimethoxysilane, triethoxyoctylsilane, tridecafluorooctyltriethoxysilane, retinyltrimethylsilane, aminopropyltriethoxysilane, preferably one or more of polymethylhydrogensiloxane, polydimethylsiloxane alcohol, triethoxyoctylsilane, tridecafluorooctyltriethoxysilane; and / or The solvent is one or more of water, ethanol, isopropanol, glycerol, and ethyl acetate, preferably one or more of pure water, ethanol, and ethyl acetate; Preferably, the mass concentration of the modifier in the modified solution is 1 to 30%, preferably 6 to 25%; and / or The mixing mass ratio of the modified solution to the mica powder is 1:3-20, preferably 1:5-15; the modified solution is added in a spraying manner under stirring, wherein the adding rate of the modified solution is 2-5 L / min.
7. The method according to any one of claims 1 to 6, characterized in that: In step 3), the heating reaction is carried out at 100 to 150° C. for 1 to 12 hours; preferably, the ambient pressure of the heating reaction is negative pressure (preferably the negative pressure is not less than -24 KPa); and / or The dispersion treatment is to use gas with a gas pressure of 0.5 to 1 MPa to perform airflow dispersion treatment while the feed rate is 1 to 5 Kg / min.
8. The method according to any one of claims 1 to 7, characterized in that: In step 3), a catalyst is further added to the modified solution, and the catalyst is one or more of hydrochloric acid, acetic acid, tartaric acid, citric acid, and 1,2-succinic acid, preferably one of hydrochloric acid, tartaric acid, and citric acid; Preferably, the catalyst is added in an amount of 0.05-2.5% of the total mass of the modified solution, preferably 0.1-2%.
9. The method according to any one of claims 1 to 8, characterized in that: The average particle size of the long-lasting synthetic mica powder is 1-10 μm, its whiteness is not less than 85, its pH value is 4.5-6.5, its water contact angle is not less than 135°, and its product activation degree is not less than 99%.
10. The method according to any one of claims 1 to 9, characterized in that: The structure of the long-lasting synthetic mica powder is as follows: synthetic mica is used as the core, and a modified molecular layer is coated on the surface of the synthetic mica; wherein the hydrophobic groups of the modified molecular layer face outward, and Si-O-Si bonding bonds are formed between the inner silicon atoms and the synthetic mica; and the surface bonding structure is as follows: Wherein, R is a hydrophobic functional group, preferably one or more of octyl, hexyl, tridecafluorooctyl, n-hexadecyl, aminopropyl, and retinyl.
Citation Information
Patent Citations
Preparation method of foundation make-up premix having minimal color difference
CN104055684A
Make-up powder-based fixing composition and preparation method thereof
CN105581923A
Method for treating and modifying synthetic mica powder used for paint
CN105925072A
Organic matter coating method of mica powder used for cosmetics
CN107337943A
Highlight synthetic mica powder for cosmetics and preparation process thereof
CN114180593A