Anti-infection GOX silk and application thereof as material for repairing diabetic chronic wounds
GOX-Fe3O4 silk hydrogels were prepared by expressing GOX in the silk glands of domestic silkworms. GOX catalyzes the production of H2O2 from glucose and the production of ·OH from Fe3O4 NPs, which solves the problem of poor efficacy of existing antibiotics and achieves effective treatment and healing of chronic infectious wounds in diabetic patients.
Patent Information
- Application Number
- CN202411032370.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
Existing antibiotics have weakened their bactericidal effect, and the development of new antibiotics is lagging behind, making it difficult to effectively treat chronically infected wounds caused by diabetes. New antibacterial strategies need to be found.
GOX silk was prepared by expressing glucose oxidase (GOX) in the silk glands of domestic silkworms. Combined with Fe3O4 nanoparticles (Fe3O4 NPs), a GOX-Fe3O4 silk hydrogel was formed. GOX catalyzes the production of H2O2 from glucose and catalyzes the production of ·OH from Fe3O4 NPs under acidic conditions, thereby enhancing the antibacterial effect.
GOX-Fe3O4 silk hydrogel significantly inhibits bacterial growth in the presence of glucose, promotes the healing of chronic infectious wounds in diabetic patients, and exhibits good biocompatibility and antibacterial activity.
Smart Images

Figure CN118949131A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the fields of engineering technology and medicine, and in particular to anti-infection GOX silk, and also to application of GOX silk as a material for repairing diabetic chronic wounds. Background Art
[0002] As people's living standards improve, the number of diabetic patients is also increasing year by year, especially obese people are more likely to suffer from diabetes. However, the risk of amputation caused by foot ulcer infection caused by diabetes is 10-20 times higher than that of non-diabetic patients. Therefore, how to effectively promote the healing of chronic combined infection wounds caused by diabetes is the focus of current research. Antibiotics are a common antibacterial agent that can be used in combination with some materials to treat infected wounds. However, due to the incorrect use of antibiotics, bacterial resistance has been generated, and the killing effect of antibiotics on bacteria has been weakened, which cannot achieve the ideal therapeutic effect. In addition, the development of new antibiotics is far behind the evolution of drug-resistant bacteria. Therefore, there is an urgent need to find a new antibacterial strategy to solve this problem.
[0003] Chemodynamic therapy (CDT) is a safe and effective antibacterial therapy. Through the Fenton reaction, intracellular hydrogen peroxide (H2O2) is converted into highly toxic hydroxyl radicals (·OH). ·OH can rupture the bacterial cell membrane and cause the contents to flow out, thus killing bacteria. Some metal nanomaterials can exhibit Fenton's catalytic activity. S ) has pH-dependent peroxidase activity (POD) and catalase activity (CAT). Under slightly acidic conditions, Fe3O4 NP S It can catalyze H2O2 to generate highly toxic ·OH, and can catalyze H2O2 to generate non-toxic water and oxygen under neutral conditions. S To produce more ·OH, we need to provide additional H2O2 and create an acidic environment. However, the H2O2 content in cells is generally very small, and the normal wound site cannot reach an acidic environment.
[0004] Glucose oxidase (GOX) is an oxidoreductase that catalyzes glucose in wound tissue to produce H2O2 and gluconic acid. Glucose oxidase (GOX) is a dimeric protein composed of two identical polypeptide chain subunits linked together by disulfide bonds. It can use molecular oxygen as an electron acceptor to specifically catalyze β-D-glucose to gluconic acid and produce H2O2 at the same time. GOX can not only consume glucose to starve bacteria, but the product H2O2 can also affect the function of bacteria by affecting the chemical oxidation of key biomolecules (lipids, proteins, and DNA), thus being applied to the treatment of wound infections. The gluconic acid and H2O2 produced by GOX catalyzing glucose can improve the catalytic efficiency of CDT. Therefore, combining GOX with CDT preparations provides a potential synergistic antibacterial treatment, which is considered to have better therapeutic effects than a single component. Wang et al. used GOX to prepare a GOX–Cu Ca / Pt nanoreactor, which has nanozymes with multiple enzyme activities (peroxidase, catalase, and glucose oxidase). In this cascade catalytic system, GOX catalyzes glucose to produce gluconic acid and H2O2, where the generated gluconic acid provides an acidic microenvironment for the reaction, and H2O2 provides a substrate for the catalytic reaction of the nanozyme. Zhang et al. incorporated GOX into the hydrogel, and the results showed that the hydrogel had good antibacterial activity, could regulate the levels of glucose and reactive oxygen species on the wound surface, and had a good therapeutic effect on chronic diabetic wounds.
[0005] The silk gland of the silkworm is an organ that synthesizes and secretes silk protein, and is the biological basis of the entire silk industry. After thousands of years of artificial domestication, the silk gland of the silkworm has a super strong ability to synthesize and secrete protein. A silkworm weighing about 5g can synthesize and secrete about 0.5g of silk protein, which is the highest among the known insects. This feature makes it an ideal bioreactor model, which has attracted the attention of researchers from all over the world and is being developed and utilized. In recent years, researchers at home and abroad have established a silk fibroin expression system and a sericin expression system based on the piggyBac transposon, and have successively conducted expression studies on dozens of exogenous proteins. Among them, the silk fibroin expression system was used to fusion express: EGFP, cat interferon, spider silk traction protein, some peptides of human type III collagen, FGF2, and RFP, etc.; the sericin system was used to recombinantly express: EGFP, mouse monoclonal antibody), human collagen α chain gene, GM-Csf receptor α, FGF1, PDGF-BB, Lactoferrin, CTGF, human superoxide dismutase 3, and human serum albumin, etc. In summary, using silkworm silk glands as bioreactors to produce exogenous proteins with high added value not only has broad market prospects, but also can break the barrier that silkworms can only be used as traditional industries, and provide a basic technical system guarantee for the development of new silkworm industries.
[0006] At the same time, silk itself is also a bio-based material with excellent mechanical properties and biocompatibility. First, the fibroin in silk has better mechanical properties than other natural fibers. It can be processed into membrane scaffolds or other forms, such as electrospinning, electrospinning membranes, gels, biofilms, microspheres and scaffolds. The surface is easy to chemically covalently modify adhesion sites and cytokines, can be biodegraded, and its degradation rate is controllable. The degradation products are not only non-toxic and side effects to the surrounding tissues, but also have a nutritional and repairing effect on the surrounding tissues. It can simulate the extracellular matrix and provide a good environment and support for cell adhesion, proliferation and differentiation into tissues. Secondly, due to its hydrophilicity, biocompatibility and biodegradability, sericin in silk has recently been considered as a potential biomaterial for biological applications. It can be made into hydrogels, films or 3D scaffolds with characteristics related to tissue engineering and regeneration. At present, the medical applications of sericin materials mainly include wound dressings, drug delivery, and repair of nerve damage. Therefore, through the silkworm silk gland biosynthesis technology, the directional design and functional genetic improvement of silk will further expand the application of silk and various synthetic exogenous proteins in the field of tissue medicine.
[0007] The present invention involves the creation of a new type of silkworm germplasm material for biosynthesizing GOX silk, and then using the obtained functional GOX silk to develop GOX and Fe3O4 NPs (GOX–Fe3O4) silk hydrogel materials. Finally, the developed GOX and Fe3O4NPs (GOX–Fe3O4) silk hydrogel is used to repair chronic diabetic wounds with infection, and its therapeutic effect and mechanism of promoting the healing of chronic diabetic wounds with infection are systematically studied. Summary of the invention
[0008] In view of this, one of the objects of the present invention is to provide anti-infection GOX silk; the second object of the present invention is to provide the use of the GOX silk in the preparation of antibacterial materials, the third object of the present invention is to provide a method for preparing a GOX silk extract; the fourth object of the present invention is to provide a method for preparing a GOX and Fe3O4 NPs silk hydrogel material; the fifth object of the present invention is to provide the use of the GOX-sericin hydrogel prepared by the method or the GOX and Fe3O4NPs silk hydrogel material prepared by the method in the preparation of materials for repairing diabetic chronic wounds.
[0009] By developing GOX and Fe3O4 NPs (GOX–Fe3O4) silk hydrogel materials, the developed GOX and Fe3O4NPs (GOX–Fe3O4) silk hydrogels were used to repair chronic diabetic infected wounds, and their therapeutic effects and mechanisms of action in promoting the healing of chronic diabetic infected wounds were systematically studied.
[0010] In order to achieve the above object, the present invention provides the following technical solutions:
[0011] 1. An anti-infection GOX silk, wherein the GOX silk is a transgenic silk obtained by expressing glucose oxidase in the silk gland of Bombyx mori mediated by the silk fibroin heavy chain promoter.
[0012] Preferably, the GOX silk is obtained by connecting the glucose oxidase coding sequence shown in SEQ ID NO.1 to the downstream of the Bombyx mori silk fibroin heavy chain promoter of the pBac-HFIRS vector, obtaining the vector for transformation microinjection, and screening transgenic silkworms. The silk secreted by the transgenic silkworms is the anti-infection GOX silk.
[0013] 2. Application of the GOX silk in the preparation of antibacterial materials.
[0014] 3. A method for preparing a GOX silk extract is to add GOX silk into a PBS solution, place the solution on a magnetic stirrer at 4-25° C. for extraction for 6-12 hours, and then collect the supernatant by centrifugation to obtain a GOX extract.
[0015] Preferably, the sericin solution is mixed with the GOX silk extract prepared by the method of claim 4, and then dialyzed at a temperature of 4-25°C for at least 3 days to obtain the GOX-sericin hydrogel.
[0016] Preferably, in the present invention, the mass fraction of the sericin solution is 16%; and the volume ratio of the sericin solution to the GOX silk extract is 1:3.
[0017] Preferably, the sericin solution and the GOX silk extract are mixed, and then the Fe3O4 NPs solution is added, and then dialyzed at a temperature of 4-25°C for at least 3 days to obtain a GOX and Fe3O4 NPs silk hydrogel material.
[0018] Preferably, the Fe3O4 NPs solution is prepared by adding Fe3O4 NPs into water at a concentration of 5 mg / ml and ultrasonicating for 30 minutes.
[0019] Preferably, in the present invention, the volume ratio of the sericin solution to the GOX silk extract is 1:3, and the concentration of the Fe3O4 NPs solution after addition is 0.1 mg / mL.
[0020] 5. Use of the GOX-sericin hydrogel prepared by the method or the GOX and Fe3O4 NPs silk hydrogel material prepared by the method in preparing materials for repairing chronic diabetic wounds.
[0021] The beneficial effects of the present invention are as follows: the present invention discloses a new type of silkworm germplasm material for creating biosynthetic GOX silk, and then utilizes the obtained functional GOX silk to develop GOX and Fe3O4 NPs (GOX–Fe3O4) silk hydrogel materials. Finally, the developed GOX and Fe3O4 NPs (GOX–Fe3O4) silk hydrogel is used to repair chronic diabetic wounds with infection, and the therapeutic effect and mechanism of promoting the healing of chronic diabetic wounds with infection are systematically studied. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to make the purpose, technical solution and beneficial effects of the present invention clearer, the present invention provides the following drawings for illustration:
[0023] Figure 1 To establish and optimize the hybrid strain of GOX-transformed silkworm (A: Schematic diagram of the vector structure for expressing GOX in the silk gland of silkworm; B: Fluorescence images of GOX-negative (right) and positive individuals (left); C: Appearance of cocoons of GOX-D9L, F1 hybrids, and F2 hybrids (silkworms selected for subsequent breeding individuals); D: Statistics of cocoon layer weights of GOX-D9L, F1 hybrids, and F2 hybrids (n=50); E: SDS-PAGE of GOX-D9L, GOX-F1, and GOX-F2 cocoon proteins; F: SEM images of different silks 10 hours after co-culture with S. aureus; G: SEM images of different silks 10 hours after co-culture with E. coli).
[0024] Figure 2 The antibacterial zone test of GOX silk (A: pictures of the antibacterial zones produced by WT cocoon pieces, GOX cocoon pieces and 3% H2O2 with S. aureus; B: diameter statistics; C: kinetic curves of the optical density changes of S. aureus cultured with different silks; D ... Image of the inhibition zone produced by H2O2 and E.coli; E: diameter statistics; F: kinetic curve of optical density change of E.coli growth cultured with different silks; G: reducing SDS-Page detection in GOX silk extract; H: non-reducing SDS-Page detection in GOX silk extract; I: bacterial growth kinetic curve of S.aureus; J: culture medium status after co-culture; K: bacterial growth kinetic curve of E.coli; L: culture medium status after co-culture; M: protein marker; 1: WT silk extract, 2: GOX silk extract, 3: GOX standard; black box: GOX monomer; red box: GOX dimer; blue arrow: sericin; black ruler: 5mm).
[0025] Figure 3Peroxidase activity of Fe3O4 NPs solution (A: UV-vis absorption curve of reactants in TMB solution and the corresponding picture of reaction solution; B: UV-vis absorption curve of Fe3O4 NPs in TMB / H2O2 solution at different pH and the corresponding picture of reaction solution).
[0026] Figure 4 To verify the enzyme catalytic function of GOX silk extract-Fe3O4 NPs ((A) The change in pH after the catalytic reaction between GOX silk extract and different concentrations of glucose; (B) The UV-vis absorption curve after the color development reaction between the Fe3O4-GOX system with different concentrations of glucose as substrate and TMB and the color development of the solution after the color development reaction).
[0027] Figure 5 Preparation of hydrogel (A: preparation flow chart and sterilization mechanism of GOX-Fe3O4 hydrogel; B: actual hydrogel and picture after freeze-drying).
[0028] Figure 6 The microstructure of the composite hydrogel (A: scanning electron microscope images of different hydrogels; B: pore size statistics of different hydrogels).
[0029] Figure 7 Infrared spectroscopic characterization of different hydrogels (A: infrared spectra of different hydrogel samples; B: amide I peak diagram of different hydrogel samples).
[0030] Figure 8 The swelling properties of the hydrogel (A: swelling kinetics curves of different hydrogel samples; B: equilibrium swelling ratios of different hydrogel samples).
[0031] Fig. 9 Biodegradation properties of hydrogels (A: degradation curves of different hydrogel samples in PBS; B: degradation curves of different hydrogel samples in trypsin solution; C: mass loss of GOX-Fe3O4 hydrogel in PBS and trypsin solution on the 1st and 7th days).
[0032] Fig.10 The enzymatic catalytic performance of the hydrogel (A: UV-vis absorption curves of the color development reaction between different hydrogels and TMB and the corresponding color development of the TMB solution; B: UV-vis absorption curves of the color development reaction between GOX-Fe3O4 hydrogel and TMB in the system with different concentrations of glucose as the substrate and the corresponding color development of the TMB solution).
[0033] Fig.11Growth inhibition curves of different hydrogel samples and bacteria (A: kinetic curve of optical density measurement change of S. aureus cultured with different hydrogel samples; B: agar plate picture of S. aureus cultured with different hydrogel samples for 10 hours; C: kinetic curve of optical density measurement change of E. coli cultured with different hydrogel samples; D: agar plate picture of E. coli cultured with different hydrogel samples for 10 hours).
[0034] Fig.12 These are scanning electron micrographs of S. aureus and E. coli after being treated with different hydrogels.
[0035] Fig.13 This is an inhibition zone test (A: inhibition zone test of hydrogel on S. aureus; B: diameter statistics of the inhibition zone of hydrogel on S. aureus; C: inhibition zone test of hydrogel on E. coli; D: diameter statistics of the inhibition zone of hydrogel on E. coli).
[0036] Fig.14 The cytotoxicity of the hydrogel (A: MTT method was used to detect the survival rate of 3T3 cells after 12 hours; B: white light image of 3T3 cells after incubation with different hydrogels for 12 hours).
[0037] Fig.15 The blood compatibility of the hydrogel (physical image scale) (A: hemolysis rate of different hydrogel material tests; B: pictures corresponding to the hemolysis rate tests of different hydrogel materials).
[0038] Fig.16 This is an infectious wound healing experiment in diabetic mice (A: animal experiment flow chart; B: representative pictures of mouse wounds in different treatment groups on days 0, 3, 7, and 12; C: traces of mouse wound closure in different treatment groups on days 0, 3, 7, and 12; D: statistics of mouse wound areas in different treatment groups on days 7 and 12; E: flat plate coating of wound exudate in different treatment groups).
[0039] Fig.17 H&E staining of mouse wound tissues on days 7 and 12 (red arrows: blood vessels; blue arrows: sebaceous glands; black arrows: hair follicles).
[0040] Fig.18 Masson staining of mouse wound tissues on days 7 and 12. DETAILED DESCRIPTION
[0041] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0042] Example 1. Germplasm creation of GOX silkworm
[0043] The amino acid sequence of the mature peptide of GOX (ec1.1.3.4) from Aspergillus niger was used as a template, and a 6×His tag was fused to the C segment. The coding sequence was optimized and designed according to the codon usage preference of Bombyx mori, and BamHI and NotI restriction sites were added to the 5′-end and 3′-end, respectively. The gene sequence was synthesized by Genscript, and the sequence is shown in SEQ ID NO.1.
[0044] The commercially synthesized GOX sequence was constructed into pBac-HFRS (Patent Publication No.: CN113621650A) through BamHI and NotI restriction sites to form a transgenic expression vector pBac[3xp3DsRed; hr3CQ-FibHp-GOX-Ser1PA], referred to as phFGOXSer1( Figure 1 , A).
[0045] The transgenic expression vector phFGOXSer1 and the auxiliary vector pHA3PIG plasmid were extracted using the QIAGEN Plasmid Mini Kit plasmid extraction kit, and the concentration of each plasmid was diluted to 300-500 ng / μL, and mixed with the auxiliary vector pHA3PIG plasmid at a molar ratio of 1:1. The mixed plasmids were injected into early embryos of Dazao that had been released from diapause (2-5 hours after egg laying), and then the injection holes were sealed with non-toxic glue. After being sterilized with 35% formaldehyde steam for 5 minutes, the embryos were placed in an environment of 25°C and 85% relative humidity for incubation. The hatched larvae (G0 generation) were raised with artificial feed, and self-crossed or backcrossed to produce seeds after they became adults. The G1 generation silkworm eggs (day 6-7) obtained were examined under a macroscopic stereo fluorescence microscope (Olypus MVX10, Japan). The red fluorescence observation was performed with an excitation light of 510-550nm, and the green fluorescence observation was performed with an excitation light of 460-490nm. The transgenic positive moth circle that specifically excited red fluorescence in the eyes or nerves was screened out and named sgGOX ( Figure 1 , B). The statistics of fluorescence screening of transgenic silkworms are shown in Table 1, where a total of 2 positive moth circles were screened from 16 G1 moth circles, with a positive rate of 12%.
[0046] Table 1. Statistics of microinjection and fluorescence screening of GOX gene-transfected silkworms
[0047]
[0048] In order to obtain a practical strain of GOX silkworms with better economic traits, heavy cocoons, and white color, we hybridized the GOX-D9L silkworm strain with the cotton cocoon strain to obtain the GOX (F1) generation. The F1 generation individuals were raised until they formed cocoons, and the F1 generation hybrids were selected for self-pollination with high GOX protein expression, heavy cocoons, and white and plump cocoons. The above process was repeated continuously. The results showed that the F1 generation hybrid cocoon had a larger appearance and a significantly reduced pigment content. In the F2 generation, individuals with heavy cocoons and white cocoons were obtained ( Figure 1 , C). The statistical results of the cocoon weight of 50 random silkworm individuals showed that the average cocoon weight of the original GOX-D9L strain was 0.04948±0.01164g, the average cocoon weight of the F1 generation hybrid was 0.1668±0.02863g, and the average cocoon weight of the F2 generation hybrid was 0.1680±0.03774g. The cocoon weight of the F2 generation hybrid increased by 2.4 times compared with the original GOX-D9L strain ( Figure 1 , D). The SDS-PAGE results of individual cocoon proteins of GOX-D9L silkworm strain, F1 hybrid, and F2 hybrid showed that the expression of GOX protein was different between different individuals of F1 hybrid and F2 hybrid. The individuals with high protein expression were selected for hybrid breeding ( Figure 1 , E).
[0049] Example 2: Antibacterial properties of GOX silk
[0050] GOX can catalyze glucose to produce H2O2, and H2O2 can kill bacteria. Therefore, it is speculated that silk expressing GOX through the silk gland bioreactor of the silkworm can show good antibacterial effect in the presence of glucose. In this experiment, S. aureus (Gram-positive bacteria) and E. coli (Gram-negative bacteria) were selected to verify the antibacterial properties of GOX silk.
[0051] First, in order to observe the adhesion of S.aureus and E.coli on WT silk and GOX silk, 4% paraformaldehyde was used to fix the cocoon pieces after co-culture with S.aureus and E.coli for 10 hours, and the adhesion and morphological changes of S.aureus and E.coli on silk were observed by scanning electron microscopy. The experimental results after co-culture with S.aureus suspension showed that a large amount of S.aureus adhered and aggregated on the WT cocoon pieces, with a complete structure and a spherical shape; while only a very small amount of S.aureus adhered to the GOX cocoon pieces, and the structure was broken and irregular ( Figure 1, F), which indicates that GOX cocoon sheets produced a large amount of H2O2 in the presence of 5mM glucose concentration, and H2O2 played a role in killing S. aureus. Similarly, after the silk samples were co-cultured with E. coli for 10 hours, it was found that there were more E. coli attached to the WT cocoon sheets, and their structures were regular and complete, in the shape of long rods, while only a small amount of E. coli adhered to the GOX cocoon sheets, and some of the morphological structures had changed significantly, with the cell membrane shrinking and ruptured, and the contents flowing out, and no longer having their own complete structure ( Figure 1 , G). The results of scanning electron microscopy showed that GOX cocoon sheets produced H2O2 through catalytic reaction in the presence of 5 mM glucose concentration, and H2O2 destroyed the morphological structure of S. aureus and E. coli, causing S. aureus and E. coli to die due to oxidation.
[0052] Subsequently, the antibacterial activity of GOX cocoon pieces was detected by the pre-inoculation plate method. A common disinfectant on the market (3% H2O2) was used as a positive control. 5mm-diameter round WT cocoon pieces, GOX cocoon pieces, and filter paper pieces with 3% H2O2 added were placed on a solid plate containing 5mM glucose, and the test results were observed after overnight incubation. On the solid plate containing S. aureus, it can be seen that the WT cocoon pieces did not produce an inhibition zone, while the diameter of the inhibition zone produced by the GOX cocoon pieces was 13.71±0.5597mm, and the diameter of the inhibition zone produced by the filter paper piece with 3% H2O2 added was 13.65±1.066mm. The inhibition zones produced by the GOX cocoon pieces and the filter paper pieces with 3% H2O2 were similar in size ( Figure 2 , B), but the inhibition zone produced by GOX cocoon sheets was clearer than that produced by 3% H2O2, and it could still maintain an obvious inhibition range after 72h ( Figure 2 , A). This indicates that GOX cocoon sheets can catalyze glucose to produce H2O2 on a solid plate containing 5mM, and the produced H2O2 exerts its bactericidal effect of chemical oxidation, killing bacteria and producing an inhibition zone; similarly, the antibacterial results of the solid plate added with E.coli also produced similar results. The diameter of the inhibition zone produced by the GOX cocoon sheets was 8.737±1.407mm, and the diameter of the inhibition zone produced by the filter paper with 3% H2O2 added was 8.457±1.351mm. The size of the inhibition zone produced by the GOX cocoon sheets and the filter paper with 3% H2O2 added was similar, and the edge of the inhibition zone was relatively clean ( Figure 2 , D and E). The results of the inhibition zone test showed that GOX silk had a good antibacterial effect on S. aureus and E. coli in the presence of low concentration of glucose (5 mM).
[0053] Finally, the antibacterial properties of GOX silk were verified using bacterial growth curves in liquid LB medium containing 5 mM glucose. The first group was a blank control without any silk sample, the second group contained WT cocoon pieces with a diameter of 5 mm, and the third group contained GOX cocoon pieces with a diameter of 5 mm, with other conditions being the same. From the bacterial growth curves with the S. aureus suspension, it can be seen that the absorbance values of S. aureus bacteria in the blank control group and the WT silk group showed the same trend of change, while the absorbance value of S. aureus bacteria in the GOX silk group did not increase ( Figure 2 , C), indicating that GOX silk can use the glucose in the culture medium to produce bactericidal H2O2 and inhibit the growth of S. aureus. After different silk samples were co-cultured with S. aureus suspension for 10 hours, the culture medium of the blank control and WT silk group became turbid, while the GOX silk group remained clear ( Figure 2 , C). After that, the bacterial suspension after co-culture with S. aureus for 10 hours was diluted a certain multiple and then plated. The results showed that the number of S. aureus colonies in the GOX silk group was significantly reduced compared with the blank control and WT silk group, which further showed that GOX silk had antibacterial activity in the presence of low concentration of glucose (5mM). The inhibitory effects of different silks on E. coli had similar results to S. aureus ( Figure 2 , F), GOX silk can inhibit the growth of E. coli in the presence of 5mM glucose. In conclusion, GOX silk has the ability to inhibit bacterial proliferation in the presence of low concentrations of glucose (5mM), whether it is S. aureus or E. coli.
[0054] Example 3. Preparation of Glucose Oxidase (GOX) Silk Extract
[0055] The above research results show that GOX silkworm cocoons have good antibacterial activity, but because the silkworm cocoon is a closed ellipse, the silk fibers are randomly interwoven and stacked together to form a dense structure, so it is very challenging to use the silkworm cocoon directly in wound dressings. In contrast, converting silk into a hydrogel form will greatly increase its application range and use value, so we extracted the active ingredients in GOX silk and used them to prepare composite hydrogels.
[0056] GOX silk extract was prepared by PBS extraction. The specific method is as follows: GOC silk was added to PBS solution at 3% (w / v), placed on a magnetic stirrer at 4-25°C for extraction for 6-12 hours, and then centrifuged at 4°C and 12000g for 15 minutes to collect the supernatant to obtain GOx extract. The protein components in the GOX extract were detected by reducing protein gel, and it was found that in addition to the target protein GOX being extracted, a small amount of sericin was also extracted ( Figure 2 , G); The results of non-reducing protein gel showed that the GOX protein in the extract was in the form of dimers ( Figure 2 , H); BCA detected the GOX protein content in the GOX silk extract to be 0.14 mg / mL, and calculated that 7 mg of GOX protein could be extracted from 1g of GOX silk. Subsequently, the antibacterial activity of the extract was tested, and the bacterial growth kinetic curves of S. aureus and E. coli showed that the absorbance values of the GOX silk extract and the GOX standard did not increase, while the blank control showed a normal bacterial growth trend ( Figure 2 , I and K). Moreover, the liquid culture medium after 24h co-culture of GOX silk extract and GOX standard with S. aureus and E. coli was clear, while the blank control was completely turbid ( Figure 2 , J and L). The results showed that the GOX silk extract showed the same antibacterial activity as the GOX standard.
[0057] Example 4. Preparation and characterization of GOX-Fe3O4 sericin hydrogel
[0058] In recent years, iron-based antibacterial materials have been widely used. They have peroxidase activity and can catalyze H2O2 to produce ·OH, which has a better bactericidal effect. However, in practical applications, the catalytic efficiency of iron-based nanomaterials is limited because of the high pH of the reaction site and the low H2O2 content in the infection site. GOX can just react with glucose in the infection site to produce gluconic acid to reduce the pH of the wound surface and provide H2O2 to solve this problem, thereby accelerating the reaction rate. Hydrogel is a three-dimensional polymer network that is cross-linked by physical interaction or covalent cross-linking. Compared with traditional wound dressings, hydrogel can maintain the moisture of the wound environment, prevent cell dehydration, and establish a protective barrier at the wound interface to promote wound healing. It also has good biocompatibility, is more convenient to replace, reduces secondary trauma and reduces the risk of wound infection. This has made the development of hydrogel wound dressings a hot topic in the field of modern medicine in recent years. Sericin is a natural biomacromolecule material derived from silk. It has excellent biocompatibility, low immunogenicity, and the ability to promote cell adhesion and deliver drugs. Sericin-based hydrogel wound dressings have been widely studied in recent years.
[0059] (1) Preparation and properties of Fe3O4 NPs solution
[0060] a. Preparation of Fe3O4 NPs solution
[0061] Weigh 5 mg of Fe3O4 NPs into a 1.5 mL centrifuge tube, add 1 mL of ddH2O, and sonicate for 30 min to prepare a 5 mg / mL Fe3O4 NPs solution.
[0062] b. The peroxidase activity of Fe3O4 NPs solution was evaluated by the color development reaction of TMB. TMB can form a blue oxidation product under the action of ·OH, with a characteristic absorption peak at 652 nm.
[0063] c. Set up the following experimental groups: ρFe3O4, ②H2O2, ③Fe3O4-H2O2, and prepare the reaction system according to (Table 2), wherein the pH of the phosphate buffer (pH=4) is 4.0, the concentration of the Fe3O4 nano solution is 5 mg / mL, the concentration of H2O2 is 1 M, and the concentration of the TMB solution is 100 mM. Finally, the concentration of the Fe3O4 NPs solution in the system is 0.1 mg / mL, the concentration of H2O2 is 5 mM, and the concentration of TMB is 1 mM.
[0064] Table 2. Peroxidase activity of Fe3O4 NPs. Preparation of reaction systems for each group
[0065]
[0066] d. React at 37°C for 30 minutes, record the color change with a camera, centrifuge at 10,000 rpm / min for 3 minutes, take the supernatant, add 100 μL of the supernatant to each well of a 96-well plate, and measure the absorption spectrum in the wavelength range of 500-700 nm with an ELISA reader. The results are as follows: Figure 3 As shown in A. The results show that when only Fe3O4 NPs exist, TMB cannot be catalyzed to form blue oxidation products; pure H2O2 has a certain oxidizing property, producing a trace amount of light blue substances, and there is a weak characteristic absorption peak at 652nm, indicating that a very slight oxidation reaction has occurred. In contrast, when Fe3O4 NPs and H2O2 exist at the same time, the solution color is the bluest, and there is an obvious characteristic absorption peak at 652nm. The results show that Fe3O4 NPs can effectively catalyze H2O2 to cause TMB to undergo a significant color reaction.
[0067] e. In order to explore the pH dependence of the peroxidase activity of Fe3O4 NPs solution, the reaction system ③ in (Table 3) was selected, the PB buffer in ③ was replaced with PB buffers of different pH (3, 4, 5, 6, 7), and the reaction system was prepared according to Table 4.
[0068] Table 3. Peroxidase activity of Fe3O4 NPs. Preparation of reaction systems in each group
[0069]
[0070] f. After the preparation is completed, react at 37°C for 30 minutes, use a camera to record the color change, centrifuge at 10,000 rpm / min for 3 minutes, take the supernatant, add 100 μL of the supernatant to each well of a 96-well plate, and measure the absorption spectrum in the wavelength range of 500-700 nm with an ELISA reader. The results are as follows Figure 3 As shown in B. The results showed that the peroxidase activity of Fe3O4 NPs was the strongest at pH = 3, and when the pH reached above 5, Fe3O4 NPs had almost no peroxidase activity.
[0071] (2) Verification of in vitro enzyme catalytic performance
[0072] a. In order to verify whether the combination of GOX silk extract and Fe3O4 NPs can react with glucose in vitro, reduce the solution pH, and then promote Fe3O4 NPs to catalyze H2O2 to produce ·OH. Five groups of experiments were set up to simulate the normal physiological glucose concentration to the high glucose concentration of hyperglycemic patients, with glucose concentrations of 0mM, 5mM, 10mM, 15mM, and 20mM, respectively. The reaction system was prepared according to (Table 4), in which the concentration of Fe3O4 nano solution was 5mg / mL, the concentration of H2O2 was 1M, and the concentration of TMB solution was 100mM. Finally, the concentration of Fe3O4 nano solution in the reaction system was 0.1mg / mL, the concentration of TMB was 1mM, and the concentration of glucose was 0mM, 5mM, 10mM, 15mM, and 20mM, respectively.
[0073] Table 4. GOX silk extract-Fe3O4 NPs configuration system
[0074]
[0075]
[0076] b. After preparation, react at 37°C for 3 hours, use a camera to record color changes, centrifuge at 10,000 rpm / min for 3 minutes, take the supernatant, add 100 μL of supernatant to each well of a 96-well plate, and measure the absorption spectrum in the wavelength range of 500-700 nm with an enzyme marker.
[0077] c. In order to further reflect the reaction conditions in the GOX silk extract-glucose system, the pH value change in the GOX silk extract-glucose system was tested, and a glucose concentration gradient of 0mM, 5mM, 10mM, 15mM, and 20mM was set, and the reaction system was prepared according to (Table 5).
[0078] d. Use a pH meter to monitor the pH changes in the system at 1, 2, and 4 hours respectively.
[0079] Table 5. GOX silk extract-glucose preparation system
[0080]
[0081] The results are as follows Figure 4 As shown in A, the results show that the pH of the solution dropped rapidly in the first hour, and the rate of drop was related to the glucose concentration. The higher the glucose concentration, the faster the pH of the GOX silk extract dropped. In the 4th hour, the pH of the GOX silk extract dropped to about 4.0. The results show that the GOX silk extract can effectively reduce the pH of the environment in the presence of glucose, providing an acidic environment for the peroxidase activity of Fe3O4 NPs. It was verified whether a cascade reaction can occur when the GOX silk extract and the Fe3O4 NPs solution coexist in a solution containing glucose, that is, whether the H2O2 produced by GOX catalyzed by glucose can be catalyzed by Fe3O4 NPs to produce ·OH. The experimental results show that GOX and Fe3O4 NPs underwent a cascade reaction in vitro to produce ·OH, and as the glucose concentration increased, the absorption peak and the blue color produced by the reaction showed a concentration-dependent relationship with the glucose concentration ( Figure 4 , B).
[0082] (3) Preparation of high concentration sericin solution
[0083] a. Cleaning of WT cocoons: peel off the dirty impurities on the outside of the WT cocoons, use a knife to cut the cocoons open, pour out the silkworm pupae, then use tweezers to peel off the inner layer and cut the cocoons into 2 pieces.
[0084] b. Preparation of high-concentration sericin solution: Weigh 9 g of cleaned WT cocoons into a beaker, add 100 mL of 8 M urea solution thereto, cover the beaker with aluminum foil, place it in a water bath, set the temperature to 80°C, extract for 30 min, mix the WT cocoons with a glass rod every 10 min, filter out the WT cocoons after 30 min, and obtain a 9% sericin solution. Add 7 g of WT cocoons to the 9% sericin solution again, extract at 80°C for 30 min, mix the cocoons with a glass rod every 10 min, filter out the WT cocoons after 30 min, and finally obtain a high-concentration sericin solution with a bath ratio of 16%.
[0085] (4) Preparation of composite hydrogel
[0086] a. Pour the obtained 16% high concentration sericin solution into a 10 mL centrifuge tube, centrifuge at 10000 rpm / min for 10 min, and pour out the supernatant into a 50 mL centrifuge tube;
[0087] b. Preparation process of four different types of hydrogels: ① Mix a high concentration of WT sericin solution with a double distilled water solution at a ratio of 1:3 to obtain a mixture of WT sericin solution. ② Mix a high concentration of WT sericin solution with a GOX silk extract at a ratio of 1:3 to obtain a mixture of GOX extract and high concentration sericin solution. ③ Add 2 mL of 5 mg / mL Fe3O4 NPs solution to the mixtures ① and ②, respectively, to obtain a high concentration WT sericin solution mixture containing 0.1 mg / mL Fe3O4 NPs and a GOX sericin solution mixture. The above four mixtures (WT-sericin, WT-sericin-Fe3O4 NPs, GOX-sericin, and GOX-sericin-Fe3O4 NPs) were added to a dialysis bag, and the dialysis bag was placed in double distilled water after clamping the upper and lower ends with a clamp, and dialyzed in a refrigerator for 3 days, with the dialysate replaced every 12 hours.
[0088] c. After 3 days of dialysis in the refrigerator, the solution gradually gelled during the dialysis process. From the actual pictures of the hydrogel and the pictures after freeze-drying, it can be seen that the color of the hydrogel with added Fe3O4 NPs is grayish and the color distribution is uniform. The Fe3O4 NPs are evenly distributed in the hydrogel during the dialysis process ( Figure 5 , A). Subsequently, the hydrogel was taken out and a picture of the hydrogel was taken. The hydrogel was freeze-dried using a freeze dryer and a picture of the freeze-dried material was taken ( Figure 5 , B).
[0089] (5) Microstructure of hydrogel
[0090] a. Sample preparation: Four types of hydrogel materials were prepared.
[0091] b. Cut the obtained hydrogel material into small pieces and place them in a centrifuge tube. Wrap them with lens paper and cool them in liquid nitrogen. After cooling, place the centrifuge tube in a freeze dryer and take it out after freeze drying for 2 days.
[0092] c. Take out the freeze-dried sponge material and use a blade to cut uniform sheets of material from the sponge. During this process, be careful not to press the material to cause it to deform.
[0093] d. Stick conductive glue on the sample stage, stick the sheet material to the conductive glue, and then take the sample stage for gold spraying for 120 seconds.
[0094] e. Place the sample stage under a scanning electron microscope and observe and take pictures.
[0095] Scanning electron microscopy results showed that the four prepared hydrogels all had a porous network structure ( Figure 6 , A), the results show that the addition of Fe3O4 NPs did not cause changes in the microstructure of the hydrogel. The pore size statistics of the four hydrogels using image J software showed that the average pore size of WT hydrogel was 58.44μm, the average pore size of WT-Fe3O4 hydrogel was 54.52μm, the average pore size of GOX hydrogel was 66.11μm, and the average pore size of GOX-Fe3O4 hydrogel was 61.3μm. The pore sizes of these four hydrogels were mainly distributed between 30-90μm ( Figure 6 , B), this porous mesh structure is conducive to the release of drugs, can provide enough space for cell growth, and can effectively absorb the exudate from the wound site, maintain a moist microenvironment of the wound, and is conducive to gas exchange with the outside world. The pore size of sericin hydrogel is an important evaluation index in practical applications. Different pore sizes are suitable for culturing different types of cells. The pore size of 20-125μm is suitable for the regeneration of skin tissue. The pore sizes of the four hydrogels prepared in this study are within this range, indicating that they will promote the repair of skin tissue.
[0096] (6) FTIR determination of the secondary structure of hydrogel
[0097] Generally speaking, the secondary structure of the hydrogel determines its function. The C=O stretching vibration of the amide group forms the amide I absorption peak, the NH bending and CH stretching vibration form the amide II absorption peak, and the NH in-plane bending vibration coupled with the CN stretching vibration forms the amide III absorption peak. Among them, the amide I absorption peak is most commonly used to evaluate the secondary structure of the hydrogel, which is mainly located at 1700cm -1 -1600cm -1 area.
[0098] a. The four hydrogels prepared above were freeze-dried to prepare sponge materials.
[0099] b. Cut a very thin transparent sheet from the sponge material, collect the background first, and then put the transparent sheet into the Fourier infrared spectrometer for detection. The detection range is 4000-800cm -1 The number of scans was 256, the sample test temperature was 25°C, each sample was measured 10 times, and a group of 3 samples was analyzed and plotted. The results are as follows: Figure 7 The experimental results show that the absorption peaks of the four hydrogel amides Ⅰ, Ⅱ, and Ⅲ are close to each other, among which amide Ⅰ is located at 1620 cm -1Nearby, amide II is located at 1530 cm -1 Nearby, amide III is located at 1240 cm -1 nearby( Figure 7 , A), the addition of Fe3O4 NPs did not change the positions of the absorption peaks of amide Ⅰ, Ⅱ, and Ⅲ. -1 ) were used for peak separation, and the results showed that the peak shapes of amide I with and without Fe3O4 NPs were similar ( Figure 7 , B).
[0100] (7) Swelling behavior of hydrogel
[0101] A hydrogel with excellent swelling properties can fit closely to the wound site, absorb excess exudate from the wound site, maintain a moist microenvironment in the wound, and accelerate the wound healing process. The swelling behavior of the hydrogel can reflect its ability to absorb water. The swelling kinetic curves of the four hydrogels in PBS solution were investigated as follows:
[0102] a. The above four hydrogels are freeze-dried to prepare sponge materials.
[0103] b. The swelling performance of the hydrogel was tested by weighing method. A small piece of 3-4 mg (W0) was cut from the freeze-dried hydrogel and soaked in 4 mL PBS solution for 24 h. The hydrogel was taken out every 10 min, 30 min, 1 h, 2 h, 4 h, 8 h, 12 h, and 24 h. The sponge was placed on filter paper and rolled until there was no water mark and then weighed (W1). The swelling rate was calculated as follows:
[0104] Swelling rate = (W1-W0) / W0×100%
[0105] The results are as follows Figure 8 As shown. The results show that the four hydrogels have similar swelling kinetics curves. They absorb a large amount of water rapidly in the early stage, reaching about 1000% in the tenth minute, and then the water absorption rate slowly decreases, and the swelling rate reaches about 2000% in the 24th hour. Zhang et al. prepared a new self-assembled hydrogel by grinding and high temperature and high pressure. The volume of the hydrogel increased sharply during the first 12 hours of immersion, and then slowly expanded, which is similar to the swelling kinetics results of our sericin hydrogel.
[0106] (8) Porosity calculation
[0107] The porosity of scaffold materials plays an important role in guiding the formation and function of tissues. It can ensure the connection and uniform distribution of cells in tissue engineering, promote the transport of nutrients and oxygen diffusion, and promote local angiogenesis in some tissues lacking blood vessels. The porosity of four hydrogels was tested using the liquid replacement method. Add 4mL ddH2O to a 10mL centrifuge tube, record the volume at this time (V0), add different freeze-dried hydrogels to the centrifuge tube, and after 1h, record the volume in the tube at this time (V1). After taking out the hydrogel, record the remaining volume in the centrifuge tube (V2). The porosity calculation formula is as follows:
[0108] Porosity = (V0-V2) / (V1-V2)×100%
[0109] The porosity calculation results are shown in Table 6. The results showed that there was no significant difference in porosity among the four hydrogels, and the higher porosity showed that the hydrogel had the potential to promote skin wound repair.
[0110] Table 6. Pore size and porosity of freeze-dried composite hydrogel samples
[0111]
[0112] (9) Biodegradability of hydrogel
[0113] The mass loss of the freeze-dried hydrogel material in the solution (PBS and PBS solution containing trypsin) was counted to characterize the biodegradability. The specific method is as follows:
[0114] a. Prepare 4 kinds of freeze-dried hydrogel sponge materials according to the above method.
[0115] b. After preparation, cut the sponge material into small pieces of about 3-4 mg, weigh them using a 1 / 10,000 balance and record their weight, which is recorded as W0.
[0116] c. Place the weighed sponge materials into a 24-well plate in turn, then add 1 mL of PBS solution and PBS solution containing 0.3 mg / mL trypsin into the wells respectively, store at room temperature, aspirate the solution in the 24-well plate at 1d, 2d, 3d, 4d, 5d, 6d, and 7d respectively, rinse slowly with deionized water 3 times, seal with plastic wrap, and use a needle to poke some small holes in the plastic wrap, place the 24-well plate in liquid nitrogen to cool, and then freeze-dry. After 48h, weigh the weight of the freeze-dried sponge and record it as W1.
[0117] d. The weight loss rate is calculated as follows: (W1-W0) / W0×100%
[0118] The results are as follows Fig. 9The results showed that within 7 days, the mass loss curves of the four freeze-dried hydrogel materials were similar, regardless of whether the materials were in PBS solution or trypsin solution. The addition of Fe3O4 NPs did not affect the in vitro degradation rate of the hydrogels, and the four prepared hydrogels were all degradable. The degradation of the hydrogels in PBS solution was relatively mild ( Fig. 9 , A). In the PBS solution containing trypsin, the hydrogel degradation rate was faster in the early stage, and the hydrogel degradation was fastest on the first day, and the degradation rate slowed down after 3 days ( Fig. 9 , B). After 7 days, the GOX-Fe3O4 hydrogel lost 25.16% of its mass in PBS solution and 59.16% of its mass in trypsin solution. The mass loss of the hydrogel in the enzyme solution was significantly higher than that in the PBS solution ( Fig. 9 , C). The reason may be that trypsin can selectively cleave the peptide bonds on the carboxyl side of arginine or lysine, and sericin contains a high content of lysine and arginine, so trypsin degrades sericin hydrogel faster.
[0119] (10) Secondary structure content of hydrogel
[0120] The secondary structure contents of the four hydrogels were statistically analyzed, and the results showed that the secondary structure contents of the four hydrogels were similar, and the addition of Fe3O4NPs did not cause changes in the secondary structure of the hydrogels. Among them, the β-folding content of GOX-Fe3O4 hydrogel was 33.4%, the random curling content was 30.59%, the α-folding content was 23.44%, and the β-turn content was 12.57% (Table 7). The hydrogel has a higher β-folding content, indicating that sericin forms a more stable cross-linked network during dialysis.
[0121] Table 7. Secondary structure analysis of sericin hydrogel
[0122]
[0123] Example 5. Biological functions of GOX-Fe3O4 hydrogel
[0124] (1) Determination of enzyme catalytic performance of hydrogels
[0125] TMB solution was used to evaluate whether the prepared hydrogel could decompose H2O2 to produce ·OH, so that the colorless TMB solution was oxidized into blue ox TMB with a characteristic absorption peak at 652 nm; five groups were set up, including ρ control, ②WT hydrogel group, ③WT-Fe3O4 hydrogel, ④GOX hydrogel, and ⑤GOX-Fe3O4 hydrogel. The reaction system was prepared according to (Table 8), wherein the pH of the phosphate buffer was 4.0, the addition amount of each hydrogel was about 30 mg, the concentration of H2O2 was 1 M, and the concentration of the TMB solution was 100 mM, so that the content of the hydrogel in the system was 30 mg / mL, the concentration of H2O2 was 5 mM, and the concentration of TMB was 1 mM.
[0126] Table 8. Configuration table of each group of reaction systems
[0127]
[0128]
[0129] The reaction was carried out at 37°C for 12 hours, and the color change was recorded by a camera. The supernatant was collected by centrifugation at 10,000 rpm / min for 3 minutes, and 100 μL of the supernatant was added to each well of a 96-well plate. The absorption spectrum in the wavelength range of 500-700 nm was measured by an ELISA reader. The results are shown in Figure 2. Fig.10 The results showed that the solutions of the blank control, WT hydrogel and GOX hydrogel groups only had a weak blue color and a weak absorption peak at 652nm, while the solution of the hydrogel group with added Fe3O4 NPs was more obvious in blue and had a stronger characteristic absorption peak at 652nm. The results showed that the hydrogel with added Fe3O4 NPs also had peroxidase-like activity ( Fig.10 , A).
[0130] (2) Verification of the GOX-Fe3O4 hydrogel cascade reaction
[0131] In order to further explore whether GOX-Fe3O4 hydrogel can use GOX to catalyze glucose to produce gluconic acid and H2O2 in the presence of glucose in vitro, and then promote Fe3O4 NPs to exert peroxidase-like activity, decompose H2O2 to produce ·OH, and oxidize TMB to blue oxidation products, we used glucose solutions of different concentrations to verify its cascade reaction rate.
[0132] The following experimental groups were set up: the glucose concentrations were set to 0mM, 5mM, 10mM, 15mM, and 20mM respectively, and the reaction system was prepared according to (Table 9), wherein the addition amount of GOX-Fe3O4 hydrogel was 30mg, the concentration of glucose was 1M, and the concentration of TMB solution was 100mM. Finally, the concentration of GOX-Fe3O4 hydrogel in the reaction system was 30mg / mL, the concentration of TMB was 1mM, and the concentrations of glucose were 0mM, 5mM, 10mM, 15mM, and 20mM respectively.
[0133] Table 9. GOX-Fe3O4 hydrogel-glucose reaction system preparation table
[0134]
[0135] The solution was reacted at 37℃ for 24h, and the color change was recorded by camera. The solution was centrifuged at 10000rpm / min for 3min, and the supernatant was taken. 100μL of the supernatant was added to each well of a 96-well plate, and the absorption spectrum in the wavelength range of 500-700nm was measured by microplate reader. The results showed that the color of the solution without glucose did not change significantly, and there was no characteristic absorption peak at 652nm, while the solution with glucose had different degrees of color change, among which the 20mM glucose solution was the bluest, and the characteristic absorption peak at 652nm was the largest ( Fig.10 , B). The results show that the 20 mM glucose group can produce more ·OH, that is, with the increase of glucose concentration, the cascade reaction speed will be faster and more ·OH can be produced, which indicates that GOX-Fe3O4 hydrogel can play a stronger bactericidal effect in an environment with higher glucose content, and may promote the healing of diabetic infectious wounds.
[0136] Example 6. Antibacterial properties of hydrogels
[0137] (1) Bacterial growth kinetics curve
[0138] a. Set up five groups: ① blank control group, ② WT hydrogel group, ③ WT-Fe3O4 hydrogel group, ④ GOX hydrogel group, and ⑤ GOX-Fe3O4 hydrogel group. Cut the hydrogel into small pieces of about 30 mg in size, sterilize with UV for 15 min, and set aside.
[0139] b. Prepare 10 according to the above method 8 CFU / mL of S. aureus and 10 7 CFU / mL E. coli bacterial suspension;
[0140] c. Add 4 mL of liquid culture medium to a 10 mL centrifuge tube. Add 40 μL of 1 M glucose solution to each centrifuge tube. At this time, the glucose concentration in the liquid culture medium is 10 mM. Then add 40 μL of 10 8 CFU / mL of S. aureus suspension and 40 μL of 10 7 CFU / mL of E. coli suspension, at this time the number of S. aureus in the culture medium is 10 6 CFU / mL, the number of E. coli is 10 5 CFU / mL, 3 replicates per group;
[0141] d. Add UV-sterilized hydrogel pieces into centrifuge tubes according to the above test groups, place the centrifuge tubes in a shaker, and culture at 37°C and 220 rpm / min for 10 h. Take out 100 μL of the culture medium at 3 h and place it in a 96-well plate to measure OD. 600 , use blank liquid LB medium to zero, and then measure once every 1 hour. The results are as follows Fig.11 As shown in A and C.
[0142] e. After 10 hours, take out the bacterial suspension of each group, dilute it a certain number of times, take 10 μL of the diluted bacterial suspension and spread it on a solid plate, place the plate in a 37°C incubator and culture it overnight, take out the plate the next day to observe the growth status and take pictures. The results are as follows: Fig.11 As shown in B and D.
[0143] The antibacterial activity of the hydrogel was verified by testing the bacterial growth curves of S. aureus and E. coli containing different hydrogels. From the bacterial growth curves of the hydrogel and S. aureus suspension, it can be seen that the absorbance values of the S. aureus bacterial suspension in the blank control, WT hydrogel and WT-Fe3O4 hydrogel groups showed the same upward trend, while the absorbance values of S. aureus bacteria in the GOX hydrogel and GOX-Fe3O4 hydrogel groups did not increase, indicating that GOX hydrogel and GOX-Fe3O4 hydrogel have the ability to inhibit the growth of S. aureus. After the different hydrogel samples were co-cultured with the S. aureus suspension for 10 hours, the culture medium of the blank control, WT hydrogel and WT-Fe3O4 hydrogel groups became turbid, while the culture medium of the GOX hydrogel and GOX-Fe3O4 hydrogel groups remained clear. The bacterial suspension after co-culture of different hydrogels with S. aureus for 10 hours was plated. The results showed that the number of S. aureus colonies in the GOX hydrogel and GOX-Fe3O4 hydrogel groups was significantly reduced, and the bacteria produced by the plate coating of the GOX-Fe3O4 hydrogel group was less than that of the GOX hydrogel group, indicating that the inhibitory effect of the GOX-Fe3O4 hydrogel group on S. aureus was stronger than that of the GOX hydrogel group. The inhibitory effect of different hydrogels on E. coli had similar results to S. aureus. GOX hydrogel and GOX-Fe3O4 hydrogel were able to inhibit the growth of E. coli in the presence of 10mM glucose. In short, whether it is S. aureus or E. coli, GOX hydrogel and GOX-Fe3O4 hydrogel have the ability to inhibit S. aureus or E. coli in the presence of 10mM glucose.
[0144] (2) Observation of bacterial morphology after co-culture
[0145] In order to further observe the changes in bacterial morphology after S. aureus and E. coli were co-incubated with WT hydrogel, WT-Fe3O4 hydrogel, GOX hydrogel and GOX-Fe3O4 hydrogel, the bacterial morphology was observed using a scanning electron microscope. 1 mL of liquid culture medium was taken out from each group and placed in a centrifuge tube. The culture medium was centrifuged at 8000 rpm / min for 5 min, the supernatant was discarded, and the bacterial pellet was resuspended with 1 mL of PBS buffer. The culture medium was centrifuged at 8000 rpm / min for 5 min, the supernatant was discarded, 500 μL of 4% paraformaldehyde solution was added for fixation for 30 min, and the supernatant was discarded after centrifugation at 8000 rpm / min for 5 min. 1 mL of 30%, 50%, 70%, 85% and 100% ethanol was added in sequence to further dehydrate the bacteria, and finally 1 mL of anhydrous ethanol was added for resuspending. 10 μL of the resuspended liquid was dropped on the surface of the silicon wafer. After natural air drying, the bacterial status on the silicon wafer was observed using a scanning electron microscope. The results are shown in the figure. Fig.12 As shown. The results showed that after incubation with S. aureus for 10 hours, the bacterial morphology of the Control, WT hydrogel and WT-Fe3O4 hydrogel groups was regular and circular, while the S. aureus incubated with GOX hydrogel and GOX-Fe3O4 hydrogel had lost its original morphology, with irregular surface, ruptured cell membrane, and contents flowing out, and the bacteria shrank and ruptured and died; after incubation with E. coli for 10 hours, the E. coli in the Control, WT hydrogel and WT-Fe3O4 hydrogel groups were long rod-shaped with intact cell membranes, while the E. coli incubated with GOX hydrogel and GOX-Fe3O4 had irregular morphology, destroyed cell membrane structure, contents flowing out, and shrunken and dead bacteria. The SEM results further showed that GOX hydrogel and GOX-Fe3O4 hydrogel had the ability to destroy the structure of S. aureus and E. coli and kill bacteria in the presence of 10 mM glucose.
[0146] (3) Inhibition zone test
[0147] a. Contains 10mM glucose, quantity is 10 6 Preparation of solid culture medium of S. aureus with a CFU / mL: Take out 200 mL of autoclaved solid culture medium, add 2 mL of 1 M glucose solution to each of them, and when the solid culture medium is cooled to about 50°C, add 2 mL of 10 8 CFU / mL of S. aureus bacterial suspension, cooled and set aside for use;
[0148] b. Contains 10mM glucose, quantity is 10 6 Preparation of solid culture medium for E. coli with CFU / mL: Take out 200mL of autoclaved solid culture medium, add 2mL of 1M glucose solution to each of them, and when the solid culture medium cools to about 50℃, add 2mL of 10 8 CFU / mL of E. coli bacterial suspension, cooled and set aside for use;
[0149] c. Use a puncher to prepare cylinders with a diameter of 8 mm and a height of about 3 mm from the four prepared hydrogels, set up ρWT hydrogel group, ②WT-Fe3O4 hydrogel, ③GOX hydrogel, ④GOX-Fe3O4 hydrogel four groups, ultraviolet sterilize for 15 min, and set aside;
[0150] d. Divide each plate containing S. aureus and E. coli into four areas, and place the ρWT hydrogel group,
[0151] ②WT-Fe3O4 hydrogel, ③GOX hydrogel, ④GOX-Fe3O4;
[0152] e. Place the culture medium in a 37°C incubator, then take a photo at 12h and use Photoshop to measure the diameter of the inhibition zone. The results are as follows: Fig.13 shown.
[0153] The results showed that the WT hydrogel and WT-Fe3O4 hydrogel groups did not produce an antibacterial zone on the solid plate containing S. aureus, indicating that the WT hydrogel and WT-Fe3O4 hydrogel did not have the ability to kill S. aureus. The diameter of the antibacterial zone produced by GOX hydrogel was 5.567±0.3073mm, and the diameter of the antibacterial zone produced by GOX-Fe3O4 hydrogel was 5.727±0.3963mm. The antibacterial zones produced by GOX and GOX-Fe3O4 hydrogels had clear edges and no significant difference in diameter ( Fig.13 , AB). Similarly, the WT hydrogel group and the WT-Fe3O4 hydrogel group did not produce an inhibition zone on the solid plate containing E. coli, while the diameter of the inhibition zone produced by the GOX hydrogel was only 0.59±0.046mm, and the diameter of the inhibition zone produced by the GOX-Fe3O4 hydrogel was only 0.6067±0.021mm. There was no significant difference in the diameter of the inhibition zone produced by the GOX and GOX-Fe3O4 hydrogels ( Fig.13 , CD), but the diameter of the inhibition zone produced on the solid plate of E. coli was much smaller than that produced on the solid plate of S. aureus, which indicated that the killing effect of GOX and GOX-Fe3O4 hydrogel on S. aureus was stronger than that on E. coli.
[0154] Example 7: Evaluation of biocompatibility of hydrogels
[0155] (1) Cytotoxicity test
[0156] NIH-3T3 cells with good adherent growth were digested with trypsin to obtain a cell suspension, which was counted using a cell counting plate. After obtaining the number of cells in the cell suspension, the cells were diluted to 5×10 4 / mL, add 100μL cell suspension to 96-well plate, so that each well has 5000 cells, and culture in 37℃ incubator for 24h to allow cells to adhere to the wall; prepare DMEM complete medium containing different concentrations of hydrogel, divided into PBS group, WT hydrogel group, WT-Fe3O4 hydrogel group, 0.1mg / mL GOX hydrogel group, 0.1mg / mL GOX-Fe3O4 hydrogel group; aspirate the DMEM complete medium after 24h of culture, and add DMEM complete medium containing different concentrations of hydrogel to each well. After 12h of culture, aspirate the medium, add CCK-8 solution, incubate at 37℃ for 1h, and measure OD 450 , and took pictures under white light to observe the cell morphology. Fig.14 The results showed that the number of cells in the hydrogel-treated group did not decrease significantly compared with the blank control group, and the cells in the hydrogel-treated group had similar morphology to the blank control group, both with spindle structures.
[0157] (2) Hemolysis test
[0158] a. Take mouse blood and place it in an anticoagulant tube, centrifuge at 2000 rpm for 10 min, and collect red blood cells;
[0159] b. Wash the red blood cells three times with sterile saline and prepare a 5% red blood cell suspension by dissolving 500 μL of red blood cells in 9.5 mL of sterile saline;
[0160] c. Grouping: The negative control group was 900 μL of normal saline, the positive control group was 900 μL of sterile water, and the experimental groups were 900 μL of normal saline and 50 mg of different hydrogel materials. 100 μL of red blood cell suspension was added to each centrifuge tube, and the centrifuge tubes were placed in a 37°C incubator and incubated for 2 hours;
[0161] d. Take out the centrifuge tube and centrifuge at 2000 rpm for 10 min, take a photo, pipette 100 μL into a 96-well plate, and measure the absorbance of the supernatant at 540 nm;
[0162] e. The calculation formula of hemolysis rate (%) is (ODs-ODn) / (ODp-ODn)×100% (ODn: absorbance value of negative control group; ODp: absorbance value of positive control group; ODs: absorbance value of sample group).
[0163] When red blood cells (RBCs) contact the surface of biomaterials with poor blood compatibility and release intracellular hemoglobin, hemolysis will occur. The hemolysis rate of biomaterials with good blood compatibility should be less than 5%. The hemolysis rates of WT hydrogel, WT-Fe3O4 hydrogel, GOX hydrogel and GOX-Fe3O4 hydrogel groups were 2.48%, 4.3%, 4.33% and 4.3%, respectively. The hemolysis rate was less than 5%. Compared with the negative control, there was no significant difference in the hemolysis rate of the four hydrogels ( Fig.15 , A). No hemolysis was observed in the centrifuge tube containing hydrogel ( Fig.15 , B), the hydrogel can be regarded as a biomaterial with good blood compatibility.
[0164] Example 8: Repair of diabetic infected wound surface
[0165] Construction of diabetic mouse model: The experimental animals were approved by the Animal Welfare Ethics Review Committee of Southwest University. Six-week-old SPF-grade C57 male mice were selected as experimental animals. After 7 days of adaptive feeding, the 6-week-old C57 mice were intraperitoneally injected with streptozotocin (STZ) at a dose of 180 mg / kg. After 72 hours, the fasting blood glucose concentration was measured. Mice with blood glucose concentrations exceeding 11 mmol / L indicated that the diabetic mouse model was successfully constructed and used for subsequent experiments.
[0166] (1) Wound healing test in diabetic mice
[0167] The diabetic mice were anesthetized by intraperitoneal injection of 4% chloral hydrate, and hair removal was performed after anesthesia. A circular full-thickness skin wound with a diameter of 8 mm was prepared on the back of the mice using a hole puncher. 50 μL of 10 6 The wound was covered with a S.aureus solution of CFU / mL to establish an infected wound model. After 30 minutes of bacterial infection, the sample was covered on the wound surface. The mice were randomly divided into 4 groups, namely, a blank control group, a WT hydrogel group, a GOX hydrogel group, and a GOX-Fe3O4 hydrogel group. Photos were taken with a camera on the 0th, 3rd, 7th, and 12th day of the wound to record the wound size, and the wound area was calculated using Image J. The calculation formula was At / A0 (A0: initial area; At: wound area at different time points later); for tissue staining analysis, the mice were killed on the 12th day, and skin tissue organs were collected. After the skin tissue was washed with PBS solution, it was placed in a 4% paraformaldehyde solution and fixed for more than 24 hours. Paraffin sections were made and HE and Masson staining analysis were performed to evaluate the repair effect of the hydrogel material on infected wounds. By observing the wounds on the 3rd, 7th, and 12th days ( Fig.16, A), the results showed that: on the 3rd day, the wounds of the blank control and WT hydrogel groups showed suppuration, indicating that the bacterial infection was serious, while the wounds of the GOX hydrogel and GOX-Fe3O4 hydrogel groups did not show redness or swelling, and the wounds were relatively clean; on the 7th day, the wounds of the blank control and WT hydrogel groups showed redness or swelling, indicating that there was still bacterial infection, which aggravated the inflammatory response and prolonged wound healing, while the wounds of the GOX hydrogel and GOX-Fe3O4 hydrogel groups showed no redness or swelling, and the wound area was smaller, which was speculated to have entered the wound remodeling stage ( Fig.16 , BC). Image J statistics of wound area showed that on the 7th day, 78.46% of the wound area in the blank control group did not heal, 78.21% of the wound area in the WT hydrogel group did not heal, 49.98% of the wound area in the GOX hydrogel group did not heal, and 50.68% of the wound area in the GOX-Fe3O4 hydrogel group did not heal; on the 12th day, 22.2% of the wound area in the blank control group did not heal, 23.45% of the wound area in the WT hydrogel group did not heal, 12.16% of the wound area in the GOX hydrogel group did not heal, and 11.14% of the wound area in the GOX-Fe3O4 hydrogel group did not heal ( Fig.16 , D). The wound area of GOX hydrogel and GOX-Fe3O4 hydrogel groups was significantly smaller than that of blank control and WT hydrogel groups, which indicates that GOX hydrogel and GOX-Fe3O4 hydrogel can effectively kill S. aureus in the wound site and promote wound healing. On the third day, sterile cotton swabs were used to dip into the wound exudate of the blank control, WT hydrogel, GOX hydrogel and GOX-Fe3O4 hydrogel groups. The results of the colony plating of the wound exudate showed that the blank control and WT hydrogel groups had more S. aureus growth, while the GOX hydrogel and GOX-Fe3O4 hydrogel groups had only a few bacterial growths ( Fig.16 , E), further proving that GOX hydrogel and GOX-Fe3O4 hydrogel can utilize glucose in the wound site to kill bacteria.
[0168] (2) H&E staining analysis of paraffin sections of mouse wound skin tissue
[0169] To further evaluate the healing effects of GOX hydrogel and GOX-Fe3O4 hydrogel on infected wound tissue, we performed H&E staining on wound tissues on days 7 and 12 ( Fig.17) staining. The results of H&E staining on the 7th day showed that all four groups of hydrogels had epithelialization, and inflammatory cells were observed, indicating that an inflammatory reaction occurred in the skin wound. The dermis tissue of the blank control and WT hydrogel groups was severely defective, while the dermis tissue of the GOX-Fe3O4 hydrogel group was well developed, with neatly arranged fat cells and complete structure. The largest number of venous vessels was observed, followed by the GOX hydrogel group. A large number of small venous vessels were also observed in the dermis tissue area. It is speculated that GOX hydrogel and GOX-Fe3O4 hydrogel catalyzed the reaction in the skin wound, controlled bacterial infection, and thus promoted angiogenesis and accelerated wound healing. The results of H&E staining on the 12th day showed that the epithelial tissue of the blank control and WT hydrogel groups was discontinuous, the dermis tissue was defective, the structure was incomplete, and a small number of sebaceous glands were observed. The epithelialization of the GOX-Fe3O4 hydrogel group was complete, the epithelial tissue was continuous and flat, the dermal tissue was well developed, the presence of hair follicles and sebaceous glands was observed, and the skin structure was more complete than on day 7. The epithelial tissue of the GOX hydrogel group was not completely healed, and the development of the dermal tissue was slightly worse than that of the GOX-Fe3O4 hydrogel group. The results of the H&E staining test showed that GOX hydrogel and GOX-Fe3O4 hydrogel could promote the healing of infected wounds.
[0170] (3) Masson staining analysis of mouse wound skin tissue
[0171] The results of Masson staining on the 7th day showed that collagen deposition occurred in all four groups to varying degrees. Compared with the blank control and WT hydrogel groups, the collagen deposition in the GOX hydrogel and GOX-Fe3O4 hydrogel groups was better. The results of Masson staining on the 12th day showed that there were a large number of collagen fibers in the GOX hydrogel and GOX-Fe3O4 hydrogel groups, and the collagen fibers were interwoven, while the collagen fibers in the blank control and WT hydrogel groups were disordered ( Fig.18 ). The results of Masson staining test showed that GOX hydrogel and GOX-Fe3O4 hydrogel could effectively promote collagen deposition and promote the healing of infected wounds.
[0172] In summary: This study successfully constructed the GOX silkworm D9L basic strain, and obtained a hybrid strain more suitable for large-scale development and production through hybrid breeding. It was found that GOX silk can exert good antibacterial activity in the presence of 5mM glucose, and the effective ingredients in GOX silk were extracted, verifying that the GOX silk extract has similar antibacterial activity to the GOX standard. GOX-Fe3O4 hydrogel was prepared by mixing high-concentration sericin solution, GOX silk extract, and Fe3O4 NPs solution, and it was found that it has a porous structure, excellent swelling properties and degradability. The biological function of the prepared hydrogel was verified. GOX-Fe3O4 hydrogel has the activity of two enzymes, peroxidase and glucose oxidase, and can undergo a cascade reaction in the presence of glucose to produce ·OH, with antibacterial activity and good biocompatibility, and showed excellent therapeutic effect in the treatment of infected wounds in diabetic mice. The antibacterial research on GOX silk in this project provides a foundation for its future application in the field of antibacterial silk fabrics; the preparation method of sericin hydrogel containing metal nanoparticles provides a reference for the preparation of more new sericin hydrogels; GOX-Fe3O4 sericin hydrogel promotes the healing of infectious wounds in diabetic mice, which expands the application of new silk prepared by silkworm silk gland bioreactors and provides a foundation for silk hydrogel materials to enter the biomedical field.
[0173] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. An anti-infective GOX silk, characterized by: The GOX silk is a transgenic silk obtained by expressing glucose oxidase in the silk gland of the silkworm mediated by the silk fibroin heavy chain promoter.
2. The anti-infective GOX silk according to claim 1, characterized in that: The GOX silk is obtained by connecting the glucose oxidase coding sequence shown in SEQ ID NO.1 to the downstream of the silkworm fibroin heavy chain promoter of the pBac-HFIRS vector, and then the vector is transformed and microinjected to screen transgenic silkworms. The silk secreted by the transgenic silkworms is the anti-infection GOX silk.
3. Use of the GOX silk according to claim 1 or 2 in the preparation of antibacterial materials.
4. A method for preparing GOX silk extract, characterized in that: The GOX silk was added into a PBS solution, placed on a magnetic stirrer at 4-25° C. for extraction for 6-12 hours, and then the supernatant was collected by centrifugation to obtain a GOX extract.
5. A method for preparing GOX-sericin hydrogel, characterized in that: The sericin solution is mixed with the GOX silk extract prepared by the method of claim 4, and then dialyzed at a temperature of 4-25° C. for at least 3 days to obtain a GOX-sericin hydrogel.
6. The preparation method according to claim 5, characterized in that: The mass fraction of the sericin solution is 16%; the volume ratio of the sericin solution to the GOX silk extract is 1:
3.
7. A method for preparing GOX and Fe3O4 NPs silk hydrogel material, characterized in that: The sericin solution and the GOX silk extract were mixed, and then the Fe3O4 NPs solution was added, followed by dialyzing at a temperature of 4-25°C for at least 3 days to obtain the GOX and Fe3O4NPs silk hydrogel material.
8. The method for preparing the GOX and Fe3O4 NPs silk hydrogel material according to claim 7, characterized in that: The Fe3O4 NPs solution is prepared as follows: Fe3O4 NPs are added into water at a concentration of 5 mg / ml, and ultrasonicated for 30 minutes.
9. The method for preparing the GOX and Fe3O4 NPs silk hydrogel material according to claim 7, characterized in that: The volume ratio of the sericin solution to the GOX silk extract is 1:3, and the concentration of the Fe3O4 NPs solution after addition is 0.1 mg / mL.
10. Use of the GOX-sericin hydrogel prepared by the method of claim 5 or 6 or the GOX and Fe3O4 NPs silk hydrogel material prepared by the method of claims 7 to 9 in preparing materials for repairing diabetic chronic wounds.
Citation Information
Cited By
Nano-composite gel for treating diabetic foot ulcer infectious wound and application of nano-composite gel
CN119746045A