Polylactic acid fiber filtering membrane as well as preparation method and application thereof

By forming a wrinkle-like structure on the polylactic fiber filter membrane and loading MOF materials, the dust adhesion problem is solved, the filtration efficiency and service life are improved, and high-efficiency filtration and antibacterial properties are achieved.

CN118949576APending Publication Date: 2024-11-15SHENHUA SHENDONG COAL GRP +3
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411258668.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Dust and other particles in existing polylactic fiber filter membranes are prone to adhere to the membrane surface, resulting in reduced filtration performance and shorter service cycles.

Method used

Modified polylactic fiber is used to form a wrinkled structure on the surface through electrospinning process, and MOF materials are loaded on the fiber surface and inside, improving the specific surface area and electrostatic adsorption force, and enhancing piezoelectric properties and antibacterial properties.

Benefits of technology

It has achieved efficient filtration of PM0.3 and PM2.5, with strong hydrophobicity, long service cycle, low air resistance and high antibacterial efficiency, extending the service life of the filter membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949576A_ABST
    Figure CN118949576A_ABST
Patent Text Reader

Abstract

The invention discloses a polylactic acid fiber filter membrane and a preparation method and application thereof.The polylactic acid fiber filter membrane comprises modified polylactic acid fiber, the surface of the modified polylactic acid fiber is in a wrinkle shape, and the modified polylactic acid fiber comprises a polylactic acid fiber matrix and an MOF material loaded on the polylactic acid fiber matrix; the polylactic acid fiber filtering membrane has the advantages of strong hydrophobicity, high surface potential, high antibacterial efficiency, high filtering efficiency, long service cycle and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fiber filter membranes, and in particular to a polylactic acid fiber filter membrane and a preparation method and application thereof. Background Art

[0002] Particulate matter (PM) in the air has a huge negative impact on human health and global climate. PM can be divided into coarse components (PM with a diameter of <10 μm) according to its diameter. 10 ), fine components (PM with a diameter <2.5 μm 2.5 ) and ultrafine components (UFPS with a diameter of <0.1μm), these particles can penetrate the respiratory system, cause health hazards, and have an impact on global climate and air quality. Due to their small mass, they are difficult to separate from other substances in the gas, and a filter medium is urgently needed to remove these particles.

[0003] Polylactic acid has good application prospects in the field of air filtration due to its good biodegradability. At present, polylactic acid is mostly used in combination with functional materials to obtain biodegradable filter membranes with excellent performance. However, the doping of existing functional materials will affect the physical and chemical properties of the filter membrane surface, making dust and other particles easily adhere to the membrane surface and block the pores of the membrane, which is not conducive to improving the filtration efficiency. At the same time, dust accumulates on the surface of the material, shortening the service life of the filter membrane.

[0004] Therefore, how to further improve the filtration efficiency and service life of the polylactic acid fiber filtration membrane is a technical problem that needs to be urgently solved in this field. Summary of the invention

[0005] The main purpose of the present invention is to provide a polylactic acid fiber filter membrane and its preparation method and application, so as to solve the problem in the prior art that dust and other particles are easily adhered to the membrane surface, resulting in reduced filtration performance and shortened service life.

[0006] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a polylactic acid fiber filter membrane is provided, which includes modified polylactic acid fibers, the surface of the modified polylactic acid fibers is wrinkled, and the modified polylactic acid fibers include a polylactic acid fiber matrix and a MOF material loaded on the surface and inside of the polylactic acid fiber matrix.

[0007] Furthermore, the mass ratio of the polylactic acid fiber matrix to the MOF material is (3-10):1; and / or the average particle size of the MOF material is 100-500 nm; and / or the MOF material includes at least one of a copper-based MOF material and a silver-based MOF material.

[0008] Furthermore, the diameter of the modified polylactic acid fiber is 30-240 nm, and the average pore size is 50-300 nm; and / or the thickness of the polylactic acid fiber filter membrane is 18-350 μm; and / or the specific surface area of ​​the polylactic acid fiber filter membrane is 132-470 m 2 / g; and / or, the water contact angle of the polylactic acid fiber filter membrane is ≥120°.

[0009] Furthermore, at a temperature of 25°C and a humidity of 45%, the surface potential of the polylactic acid fiber filter membrane is 7 to 10 kV; and / or, the polylactic acid fiber filter membrane has a surface potential of 7 to 10 kV for PM 0.3 and PM 2.5 The filtration efficiency is ≥97%; and / or, at a gas flow rate of 10 to 85 L / min, the air resistance of the polylactic acid fiber filter membrane is ≤120 Pa; and / or, at an optical density of 10 to 100 mW / cm 2 The antibacterial rate of polylactic acid fiber filter membrane against Escherichia coli and Staphylococcus aureus is ≥95%.

[0010] The second aspect of the present invention provides a method for preparing a polylactic acid fiber filter membrane, comprising the following steps:

[0011] Step S1, mixing MOF material, polylactic acid, a template agent and an organic solvent to obtain a spinning solution;

[0012] Step S2, electrospinning the spinning solution to obtain a fiber membrane precursor;

[0013] Step S3, soaking the fiber membrane precursor in water to remove the template agent to obtain a polylactic acid fiber filtration membrane.

[0014] Further, the mass ratio of MOF material, polylactic acid, and template agent is 1:(3-10):(2-8);

[0015] Preferably, the mass fraction of MOF material in the spinning solution is 0.1% to 2%;

[0016] Preferably, the mass fraction of polylactic acid in the spinning solution is 0.5% to 10%;

[0017] Preferably, the mass fraction of the template agent in the spinning solution is 10% to 30%.

[0018] Further, the organic solvent includes at least one of dichloromethane, chloroform, dimethylformamide, N-methylpyrrolidone, hexafluoroisopropanol, methanol, ethanol, isopropanol, and glycerol;

[0019] The template is a water-soluble polymer;

[0020] Preferably, the template comprises at least one of ethylene-vinyl alcohol copolymer, dextran, polyvinyl alcohol, polyacrylamide, and sodium polyacrylate;

[0021] Preferably, the weight average molecular weight of polylactic acid is 3×10 4 ~1.5×10 5 .

[0022] Further, the MOF material includes at least one of a copper-based MOF material and a silver-based MOF material;

[0023] The preparation method of the copper-based MOF material includes:

[0024] After mixing copper salt, trimesic acid and water, subjecting the mixture to microwave treatment, and drying, a copper-based MOF material is obtained;

[0025] The preparation method of the silver-based MOF material comprises:

[0026] The silver salt, 2-methylimidazole and an alcohol solvent are mixed, subjected to microwave treatment, and dried to obtain a silver-based MOF material;

[0027] Preferably, the mass ratio of trimesic acid to copper salt is (3-12):1;

[0028] Preferably, the mass ratio of 2-methylimidazole to silver salt is (2-8):1;

[0029] Preferably, the copper salt includes at least one of copper chloride dihydrate, copper nitrate, and copper acetate;

[0030] Preferably, the silver salt comprises at least one of silver nitrate, silver fluoride, and silver bicarbonate;

[0031] Preferably, the microwave treatment has a power of 100 W to 800 W, a temperature of 100 to 180° C., and a time of 1 to 35 min.

[0032] Furthermore, the voltage of electrospinning is 12 kV to 35 kV, the consumption rate of the spinning solution is 0.6 to 1.2 mL / h, and the receiving distance is 8 to 15 cm.

[0033] The third aspect of the present invention provides an air filter, comprising the polylactic acid fiber filter membrane of the first aspect or the polylactic acid fiber filter membrane prepared by the preparation method of the second aspect.

[0034] By applying the technical solution of the present invention, the specific surface area of ​​the polylactic acid fiber filter membrane can be increased by limiting the fiber surface to present a pleated structure, thereby reducing air resistance, so that the filter membrane has better air permeability while maintaining high-efficiency filtration. Secondly, the surface pleated structure is utilized to tightly load the MOF material on the fiber to prevent it from falling off, thereby enhancing the piezoelectric properties of the polylactic acid fiber filter membrane, improving the electrostatic adsorption force, and increasing the surface potential, so that the polylactic acid fiber filter membrane has good filtration performance and antibacterial properties; in addition, the pleated structure makes the fiber have excellent hydrophobicity, prevents dust from accumulating on the surface of the material, and can be reused to extend the service life, thereby obtaining a polylactic acid fiber filter membrane with strong hydrophobicity, high surface potential, high antibacterial efficiency, high filtration efficiency, and a long service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a SEM image of the polylactic acid fiber filter membrane in Example 1 of the present invention;

[0036] Figure 2 This is a SEM image of the Cu-MOF material in Example 2 of the present invention;

[0037] Figure 3 This is a SEM image of the polylactic acid fiber filter membrane in Comparative Example 1 of the present invention after the filtration performance test;

[0038] Figure 4 This is a SEM image of the polylactic acid fiber filter membrane in Comparative Example 2 of the present invention after filtering performance testing. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0040] As described in the background of the present invention, dust and other particles in the prior art are easily adhered to the membrane surface. In order to solve the above problem, in a typical embodiment of the present invention, a polylactic acid fiber filter membrane is provided, the polylactic acid fiber filter membrane comprises modified polylactic acid fiber, the surface of the modified polylactic acid fiber is wrinkled, and the modified polylactic acid fiber comprises a polylactic acid fiber matrix and a MOF material loaded on the surface and inside of the polylactic acid fiber matrix.

[0041] The polylactic acid fiber filter membrane of the present invention is a film formed by randomly stacking modified polylactic acid fibers, which can be specifically realized through an electrostatic spinning process.

[0042] The modified polylactic acid fiber is a continuous filament with a random orientation, thus forming a thin film with a mesh structure. The surface of the modified polylactic acid fiber is wrinkled. On the one hand, the surface wrinkled structure can increase the specific surface area of ​​the polylactic acid fiber filter membrane, reduce the air resistance, and make the filter membrane have better air permeability while maintaining high-efficiency filtration. On the other hand, the surface wrinkled structure can be used to tightly load the MOF material on the fiber to prevent it from falling off, which can enhance the piezoelectric properties of the polylactic acid fiber filter membrane, improve the electrostatic adsorption force, and increase the surface potential, so that the polylactic acid fiber filter membrane has good filtration performance and antibacterial properties; in addition, the wrinkled structure makes the fiber have excellent hydrophobicity, prevents dust from accumulating on the surface of the material, and can be reused to extend the service life, thereby obtaining a polylactic acid fiber filter membrane with strong hydrophobicity, high surface potential, high antibacterial efficiency, high filtration efficiency, and long service life.

[0043] The mass ratio of the polylactic acid fiber matrix to the MOF material is (3-10):1, for example, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1 or a range consisting of any two of them. By controlling the loading amount of the MOF material, the filtration performance and antibacterial effect of the fiber filtration membrane can be effectively guaranteed.

[0044] The MOF material can be loaded on the surface of the polylactic acid fiber matrix in a granular form or embedded in the polylactic acid fiber matrix. The granular MOF material can improve the adsorption performance of the polylactic acid fiber filter membrane, making it better used in the fields of filtration, purification and separation. In some embodiments, the MOF material is granular, and the average particle size of the MOF material is 200 to 500 nm. By limiting the average particle size of the MOF material to the above range, the surface potential and antibacterial performance of the polylactic acid fiber filter membrane can be further improved.

[0045] The present invention does not limit the specific type of MOF material. For example, in some embodiments, the MOF material includes at least one of a copper-based MOF material (Cu-MOFs) and a silver-based MOF material (Ag-MOFs). 2+ ) as metal nodes, and form coordination bonds with organic ligands (such as carboxylic acids, keto acids, etc.) to construct a highly ordered porous structure; Silver-based MOF materials are based on silver ions (Ag + ) as metal nodes, forming coordination bonds with organic ligands to construct a porous structure.

[0046] In some embodiments, the diameter of the modified polylactic acid fiber is 30 to 240 nm, for example, 30 nm, 50 nm, 100 nm, 200 nm, 240 nm or any two thereof, and the average pore size is 50 to 300 nm. By limiting the diameter and average pore size of the modified polylactic acid fiber, the air permeability and filtration performance of the polylactic acid fiber filter membrane can be further improved.

[0047] Specifically, the diameter of the modified polylactic acid fiber refers to the diameter of the cross section of a single modified polylactic acid fiber. Specifically, a scanning electron microscope can be used to observe the surface of the polylactic acid fiber filter membrane, and then the diameter of the modified polylactic acid fiber can be measured. Alternatively, a transmission electron microscope can be used to observe the cross section of the polylactic acid fiber filter membrane, and then the diameter of the modified polylactic acid fiber can be measured.

[0048] The fiber contains voids, i.e., the pores of the fiber, which can be continuous or discontinuous. The size and distribution of the pores have an important influence on many properties of the fiber, such as air permeability, filtering performance, etc. The average pore size of the fiber refers to the average value of the size of the pores in the fiber. By limiting the average pore size of the modified polylactic acid fiber, the air permeability and filtering performance of the polylactic acid fiber filter membrane can be improved. In the specific implementation process of the present invention, the pore structure of the modified polylactic acid fiber can be observed using scanning electron microscopes, transmission electron microscopes or X-ray tomography. By measuring the size of the pores and calculating their average value, the average pore size of the modified polylactic acid fiber can be obtained.

[0049] The present invention does not limit the specific parameters of the polylactic acid fiber filter membrane, as long as the above requirements are met. In some embodiments, the thickness of the polylactic acid fiber filter membrane is 18 to 350 μm, and the size of the polylactic acid fiber filter membrane can be adjusted according to actual needs to meet the application of different fields. In some embodiments, the specific surface area of ​​the polylactic acid fiber filter membrane is 132 to 470 m 2 / g, it can be understood that the polylactic acid fiber filter membrane has a higher specific surface area.

[0050] The water contact angle of the PLA fiber filter membrane is ≥120°. The water contact angle of the PLA fiber filter membrane refers to the angle formed by the droplet on the surface of the PLA fiber filter membrane. The water contact angle of the PLA fiber filter membrane can be measured by the following steps: cut the dry PLA fiber filter membrane into a rectangle, fix it on a glass slide, and then drip a known volume of deionized water onto the surface of the PLA fiber filter membrane. Use an optical contact angle meter to obtain an image, and use the angle measurement method to test the size of the contact angle. Five points are selected for each sample for testing, and the results are averaged. According to the measurement results, the surface characteristics of the PLA fiber filter membrane are analyzed. Generally speaking, a contact angle less than 90 degrees indicates hydrophilicity, greater than 90 degrees indicates hydrophobicity, and close to 180 degrees indicates extremely strong hydrophobicity.

[0051] The present invention limits the water contact angle of the polylactic acid fiber filter membrane to ≥120°, indicating that the polylactic acid fiber filter membrane has strong hydrophobicity and its surface has good non-adhesiveness, which effectively reduces the adhesion of dust and other particles on the membrane surface, thereby reducing clogging and maintaining a high filtration efficiency.

[0052] In some embodiments, at a temperature of 25°C and a humidity of 45%, the surface potential of the polylactic acid fiber filter membrane is 7 to 10 kV. By limiting the surface potential of the polylactic acid fiber filter membrane, it can better adsorb the substances to be filtered and improve the filtration efficiency. 0.3 and PM 2.5 The filtration efficiency of the polylactic acid fiber filtration membrane of the present invention is ≥97%. 0.3 and PM 2.5 The filtration efficiency of particles such as polylactic acid and lactic acid fibers is relatively high. In some embodiments, the air resistance of the polylactic acid fiber filter membrane is ≤120Pa at a gas flow rate of 10 to 85L / min. By limiting the air resistance of the polylactic acid fiber filter membrane, it has a lower air resistance at a certain gas flow rate, and can better achieve air exchange at a high filtration rate, and has higher air permeability. In some embodiments, the optical density is 10 to 100mW / cm 2 Under the condition of low temperature, the antibacterial rate of polylactic acid fiber filter membrane against Escherichia coli and Staphylococcus aureus is ≥95%. It can be understood that polylactic acid fiber filter membrane has excellent antibacterial properties and can achieve long-term service.

[0053] The surface potential of the polylactic acid fiber filter membrane is closely related to the filtration performance. In some preferred embodiments, the surface potential of the polylactic acid fiber filter membrane is 7.2-9.2 kV, and it hardly decays over time, indicating that it has extremely high long-term stability. The specific surface area of ​​the polylactic acid fiber filter membrane is 132.7-468.9 m 2 / g, indicating that the polylactic acid fiber filter membrane of the present invention has a higher specific surface area, which effectively improves the mechanical filtration performance of the fiber membrane. PM 0.3 Filtration efficiency is greater than 97%, PM 2.5 The filtration efficiency is greater than 99%, and the water contact angle is 124-142 degrees, indicating that the polylactic acid fiber filtration membrane of the present invention has good hydrophobicity.

[0054] The second aspect of the present invention provides a method for preparing a polylactic acid fiber filter membrane, comprising the following steps:

[0055] Step S1, mixing MOF material, polylactic acid, a template agent and an organic solvent to obtain a spinning solution;

[0056] Step S2, electrospinning the spinning solution to obtain a fiber membrane precursor;

[0057] Step S3, soaking the fiber membrane precursor in water to remove the template agent to obtain a polylactic acid fiber filtration membrane.

[0058] In the electrospinning process, the spinning solution is formed into a modified polylactic acid fiber precursor, which is randomly stacked to form a fiber membrane precursor. The modified polylactic acid fiber precursor includes a polylactic acid fiber matrix and MOF materials and templates embedded therein. The fiber membrane precursor is soaked in water to remove the template, and a polylactic acid fiber filter membrane is obtained. During the soaking process, the template embedded in the fiber is removed, resulting in tiny depressions on the surface of the material. These tiny depressions will produce stress distribution on the entire surface of the material, thereby inducing the fiber surface to be wrinkled.

[0059] Among them, the template agent serves as a sacrificial template. After removing the template agent, a modified polylactic acid fiber with a specific corrugated structure on the surface can be prepared. Such a surface corrugated structure helps to improve the hydrophobicity and specific surface area of ​​the polylactic acid fiber filter membrane.

[0060] Specifically, electrospinning can be implemented using an electrospinning device, which includes a nozzle. During the electrospinning process, the electrospinning device is started so that the spinning solution is ejected from the nozzle under the action of a high-voltage electrostatic field to form a charged jet stream. The jet stream is subjected to the action of electric field force, surface tension, and air resistance during flight, and the spinning solution is gradually stretched and refined, and the organic solvent is volatilized, and finally deposited on the receiving device to form a modified polylactic acid fiber precursor. In addition, during the multi-needle electrospinning process, it is necessary to collect and organize the modified polylactic acid fiber precursor. For example, the deposition density and arrangement of the modified polylactic acid fiber precursor can be controlled by adjusting the movement speed and direction of the receiving device, as well as the distance between the nozzle and the receiving device, so that the modified polylactic acid fiber precursor is randomly stacked to form a mesh fiber membrane precursor, and then the template agent is removed by soaking in water, and the polylactic acid filter fiber membrane is prepared by a sacrificial template method, and finally the polylactic acid filter fiber membrane is obtained.

[0061] The present invention utilizes electrospinning technology combined with a sacrificial template method to prepare a polylactic acid fiber filter membrane, which is beneficial for the MOF material crystals to be loaded on the fiber and not easily fall off, so that the polylactic acid fiber filter membrane has a higher surface potential and significant particle adsorption capacity. The surface wrinkled structure makes the fiber have excellent hydrophobicity and a larger specific surface area, thereby improving the filtration efficiency of the fiber membrane and having broad application prospects.

[0062] The MOF material, polylactic acid, template agent and organic solvent are mixed, and the MOF material, polylactic acid and template agent are fully dissolved or dispersed by stirring or ultrasound to form a uniform spinning solution. In some embodiments, the mass ratio of MOF material, polylactic acid and template agent is 1: (3-10): (2-8). Specifically, the mass ratio of polylactic acid to MOF material is (3-10): 1, for example, 3: 1, 4: 1, 5: 1, 6: 1, 7: 1, 8: 1, 9: 1, 10: 1 or a range consisting of any two of them. The mass ratio of polylactic acid to MOF material is (2-8): 1, for example, 2: 1, 3: 1, 4: 1, 5: 1, 6: 1, 7: 1, 8: 1 or a range consisting of any two of them. In some preferred embodiments, the mass fraction of MOF material in the spinning solution is 0.1% to 2%, for example, 0.1%, 0.5%, 1%, 1.5%, 2% or a range consisting of any two of them; the mass fraction of polylactic acid in the spinning solution is 0.5% to 10%, for example, 0.5%, 1%, 2%, 3%, 4%, 5%, 8%, 10% or a range consisting of any two of them; the mass fraction of the template in the spinning solution is 10% to 30%.

[0063] In order to achieve effective removal of the template in step S3, in some embodiments, the template is a water-soluble polymer. The present invention does not limit the specific type of raw materials, and can be adjusted according to actual needs. In some embodiments, the organic solvent includes at least one of dichloromethane, chloroform, dimethylformamide, N-methylpyrrolidone, hexafluoroisopropanol, methanol, ethanol, isopropanol, and glycerol; the template includes at least one of ethylene-vinyl alcohol, dextran, polyvinyl alcohol, polyacrylamide, and sodium polyacrylate. In some preferred embodiments, the organic solvent includes at least one of chloroform, dimethylformamide, and hexafluoroisopropanol; the weight average molecular weight M of ethylene-vinyl alcohol is w 5×10 4 ~2×10 5 , the weight average molecular weight of dextran M w 5×10 3 ~2×10 4 , the weight average molecular weight M of polyvinyl alcohol w 2×10 4 ~3×10 5 , the weight average molecular weight of polyacrylamide M w 1×10 4 ~1×10 5 , the weight average molecular weight of sodium polyacrylate is M w 5×10 4 ~1×10 6 .

[0064] The present invention does not limit the specific type of polylactic acid, for example, it can be L-polylactic acid or D-polylactic acid. In some embodiments, the weight average molecular weight M of the polylactic acid is w 3×10 4 ~1.5×10 5 ).

[0065] MOF materials can be obtained through commercial purchase or conventional preparation methods. In some embodiments, the MOF material includes at least one of a copper-based MOF material and a silver-based MOF material. Specifically, the preparation method of the copper-based MOF material includes: mixing a copper salt, trimesic acid and water, subjecting the mixture to microwave treatment, and drying to obtain a copper-based MOF material; the preparation method of the silver-based MOF material includes: mixing a silver salt, 2-methylimidazole and an alcohol solvent, subjecting the mixture to microwave treatment, and drying to obtain a silver-based MOF material. Among them, the preparation of MOF materials can be achieved by microwave assistance, and the yield can be improved. In some preferred embodiments, the power of the microwave treatment is 100W to 800W, the stirring speed is 100 to 450rpm, the temperature is 100 to 180°C, and the time is 1 to 35min. In addition, the yield of the MOF material can be improved by adjusting the amount of raw materials added. In some embodiments, the mass ratio of trimesic acid to copper salt is (3-12):1, for example 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1 or a range consisting of any two of them; the mass ratio of 2-methylimidazole to silver salt is (2-8):1.

[0066] The microwave-assisted hydrothermal synthesis of MOF materials not only shortens the reaction time, but also makes the synthesized MOF material crystals more regular, which helps to improve the antibacterial properties of polylactic acid fiber filter membranes.

[0067] In some embodiments, the particle size of the copper-based MOF material is 150-300 nm; the particle size of the silver-based MOF material is 250-400 nm.

[0068] The present invention does not limit the specific selection of raw materials. For example, in some embodiments, the copper salt includes at least one of copper chloride dihydrate, copper nitrate, and copper acetate; the silver salt includes at least one of silver nitrate, silver fluoride, and silver bicarbonate.

[0069] In addition, during the multi-needle electrospinning process, a high-voltage electrostatic field needs to be applied to charge the spinning solution. According to the properties and viscosity of the spinning solution, a suitable voltage range is selected. In some preferred embodiments, the voltage of electrospinning is 12 kV to 35 kV, and the consumption rate of the spinning solution is 0.6 to 1.2 mL / h.

[0070] In step S3, the soaking temperature is 25-45° C. and the soaking time is 1-4 hours to ensure complete removal of the template.

[0071] The receiving device of electrospinning can be a rotating drum, a flat plate or a mesh structure, etc. The distance of the receiving device will affect the deposition morphology and arrangement of the fibers. In some preferred embodiments, the receiving distance of the nozzle is 8 to 15 cm.

[0072] The third aspect of the present invention provides an air filter, comprising the polylactic acid fiber filter membrane provided by the first aspect or the polylactic acid fiber filter membrane prepared by the preparation method provided by the second aspect.

[0073] Due to the inclusion of the above-mentioned excellent performance polylactic acid fiber filter membrane, the air filter can achieve PM 0.3 and PM 2.5 It can effectively intercept particulate matter such as chlorine and can achieve long-term service.

[0074] The present application is further described in detail below in conjunction with specific examples, which should not be construed as limiting the scope of protection claimed in the present application. w 1.2×10 5 .

[0075] Example 1

[0076] The preparation method of the polylactic acid fiber filter membrane of this embodiment comprises the following steps:

[0077] Step S11, microwave-assisted synthesis of Cu-MOF: adding cupric chloride dihydrate and trimesic acid into water (the mass ratio of cupric chloride dihydrate to trimesic acid is 1:3), mixing evenly, placing in a microwave reactor for in-situ synthesis (output power 100 W, temperature 80° C., time 5 min), cooling to room temperature after the reaction, standing for 4 h, and drying to obtain Cu-MOF crystals;

[0078] Step S12, electrospinning to prepare a polylactic acid fiber filter membrane precursor: Cu-MOF, polylactic acid and polyvinyl alcohol (M w =2×10 4 ) were blended (the mass ratio of Cu-MOF to polylactic acid was 1:3, and the mass ratio of Cu-MOF to polyvinyl alcohol was 1:2), and uniformly dispersed in chloroform as an electrospinning stock solution (electrospinning voltage 12 kV, spinning solution consumption rate 0.6 mL / h, receiving distance 8 cm) to obtain a polylactic acid fiber filter membrane precursor;

[0079] Step S13, preparing a polylactic acid fiber filter membrane: using a sacrificial template method, the polylactic acid fiber filter membrane precursor prepared in step S12 is immersed in water for 1 hour to remove polyvinyl alcohol, thereby obtaining a polylactic acid fiber filter membrane.

[0080] Example 2

[0081] The preparation method of the polylactic acid fiber filter membrane of this embodiment comprises the following steps:

[0082] Step S21, microwave-assisted synthesis of Cu-MOF: copper nitrate and trimesic acid are added to water (the mass ratio of copper nitrate to trimesic acid is 1:6), mixed evenly, and placed in a microwave reactor for in-situ synthesis (output power 200 W, temperature 120° C., time 15 min, stirring speed 150 rpm), cooled to room temperature after the reaction, allowed to stand for 6 h, and dried to obtain Cu-MOF crystals;

[0083] Step S22, electrospinning to prepare a polylactic acid fiber filter membrane precursor: Cu-MOF, polylactic acid and ethylene vinyl alcohol (EVA) obtained in S21 are electrospun. w =5×10 4 ) were blended (the mass ratio of Cu-MOF to polylactic acid was 1:5, and the mass ratio of Cu-MOF to ethylene-vinyl alcohol was 1:3), and evenly dispersed in dimethylformamide as an electrospinning stock solution. Finally, the fiber filtration membrane precursor was obtained by electrospinning technology (electrospinning voltage 15 kV, spinning solution consumption rate 0.8 mL / h, receiving distance 10 cm);

[0084] Step S23, preparing a polylactic acid fiber filter membrane: using a sacrificial template method, immersing the fiber filter membrane precursor obtained in S22 in water for 2 hours to remove ethylene vinyl alcohol, thereby obtaining a polylactic acid fiber filter membrane.

[0085] Example 3

[0086] The preparation method of the polylactic acid fiber filter membrane of this embodiment comprises the following steps:

[0087] Step S31, microwave-assisted synthesis of Cu-MOF: copper sulfate and trimesic acid are added to water (the mass ratio of copper sulfate to trimesic acid is 1:8), mixed evenly, placed in a microwave reactor for in-situ synthesis (output power 400 W, temperature 140 ° C, time 18 min, stirring speed 200 rpm), cooled to room temperature after the reaction is completed, allowed to stand for 8 h, and dried to obtain Cu-MOF crystals;

[0088] Step S32, electrospinning to prepare a polylactic acid fiber filter membrane precursor: Cu-MOF, polylactic acid and sodium polyacrylate (M w =8×10 4 ) were blended (the mass ratio of Cu-MOF to polylactic acid was 1:8, and the mass ratio of Cu-MOF to sodium polyacrylate was 1:6), and finally the polylactic acid fiber filter membrane precursor was obtained by electrospinning technology (electrospinning voltage was 20 kV, spinning solution consumption rate was 1.0 mL / h, and receiving distance was 12 cm);

[0089] S33. Preparation of polylactic acid fiber filter membrane: Using a sacrificial template method, the polylactic acid fiber membrane obtained in S32 was immersed in water for 3 hours to remove sodium polyacrylate, thereby obtaining a polylactic acid fiber filter membrane.

[0090] Example 4

[0091] The preparation method of the polylactic acid fiber filter membrane of this embodiment comprises the following steps:

[0092] Step S41, microwave-assisted synthesis of Cu-MOF: copper acetate and trimesic acid are added to water (the mass ratio of copper acetate to trimesic acid is 1:10), mixed evenly, and placed in a microwave reactor for in-situ synthesis (output power 800 W, temperature 180° C., time 35 min, stirring speed 450 r / min), cooled to room temperature after the reaction is completed, allowed to stand for 10 h, and dried to obtain Cu-MOF crystals;

[0093] Step S42, electrospinning to prepare a polylactic acid fiber filter membrane precursor: Cu-MOF, polylactic acid and polyacrylamide (M w =5×10 4 ) were blended (the mass ratio of Cu-MOF to polylactic acid was 1:10, and the mass ratio of Cu-MOF to polyacrylamide was 1:8), and evenly dispersed in hexafluoroisopropane as an electrospinning solution. Finally, the electrospinning technology (electrospinning voltage was 35 kV, spinning solution consumption rate was 1.2 mL / h, and receiving distance was 15 cm) was used to obtain a polylactic acid fiber filter membrane precursor.

[0094] Step S43, preparing a polylactic acid fiber filter membrane: using a sacrificial template method, immersing the polylactic acid fiber membrane obtained in S42 in water for 4 hours to remove polyacrylamide, thereby obtaining a polylactic acid fiber filter membrane.

[0095] Example 5

[0096] The difference from Example 1 is that, in step S11, microwave-assisted synthesis of Ag-MOF: silver nitrate and 2-methylimidazole are added to ethanol (the mass ratio of silver nitrate to 2-methylimidazole is 1:4) and mixed evenly, and then placed in a microwave reactor for in-situ synthesis (output power 100 W, temperature 80°C, time 5 min), and after the reaction is completed, it is cooled to room temperature, allowed to stand for 4 hours, and dried to obtain Ag-MOF crystals; the Cu-MOF in step S12 is replaced by Ag-MOF to obtain the polylactic acid fiber filter membrane of this embodiment.

[0097] Example 6

[0098] The difference from Example 1 is that in step S12, the mass ratio of Cu-MOF to polylactic acid is 1:4.

[0099] Example 7

[0100] The difference from Example 1 is that in step S12, the mass ratio of Cu-MOF to polylactic acid is 1:9.

[0101] Comparative Example 1

[0102] The difference from Example 1 is that step S13 is omitted, and the polylactic acid fiber filter membrane precursor of step S12 is directly used as the polylactic acid fiber filter membrane of this comparative example.

[0103] Comparative Example 2

[0104] The difference from Example 1 is that the template agent polyvinyl alcohol is not added in step S12, and step S13 is omitted to obtain the polylactic acid fiber filtration membrane of this comparative example.

[0105] Test example

[0106] 1. Scanning electron microscope observation

[0107] The microstructure of the Cu-MOF crystal in Example 1 was observed by a field emission scanning electron microscope (model JSM-7900F, JEOL).

[0108] 2. Specific surface area test

[0109] The specific surface area of ​​the polylactic acid fiber filtration membrane was measured using a gas adsorption instrument (ASAP 2060, Micromeritics, USA) at 77K using the nitrogen adsorption isotherm method.

[0110] 3. Particle size test

[0111] The particle size was analyzed based on the standard method of ISO 13321, and the average particle size of Cu-MOF was tested. At least 3 parallel test samples were guaranteed for each group, and the results were averaged.

[0112] 4. Surface potential test

[0113] The surface potential of the polylactic acid fiber filter membrane was tested using a non-contact electrostatic meter (VM54XQS, Quatek, USA) at a test height of 2 cm. The temperature and humidity were constant at 25°C and 45%. 20 data points were randomly collected for each sample and the average value was taken.

[0114] 5. Filtration performance test

[0115] The polylactic acid fiber filter membrane (area 126.16cm 2) air filtration performance, the gas flow rate was set to 32L / min, and the particle size range of NaCl atomized particles produced by the aerosol generator was 0.1-10μm. At least 3 different positions of each group of polylactic acid fiber filter membranes were tested, and the results were averaged.

[0116] 6. Water contact angle test

[0117] The water contact angle of the polylactic acid fiber filter membrane was tested using a water contact angle meter (JC2000C, Shanghai Zhongchen Digital Technology Equipment Co., Ltd.). The dry polylactic acid fiber filter membrane was cut into a rectangle of 1 cm × 5 cm and fixed on a glass slide with double-sided tape. Then 5 μL of deionized water was added to the membrane surface, the image was frozen, and the contact angle was tested using the angle measurement method. Five points were selected for each sample for testing, and the results were averaged.

[0118] 7. Air resistance test

[0119] The respiratory resistance was measured using a micromanometer (AIRPRO AP800, TSI, USA), an anthropomorphic respirator and a simulated human head. The gas flow rate was set to 85 L / min, and the filter membrane was encapsulated on a simulated human head. The air pressure in the cavity composed of the filter material and the human head and the atmospheric pressure were measured and subtracted. The experiment was repeated three times and the average value was taken to calculate the respiratory resistance, i.e., air resistance, of the polylactic acid fiber filter membrane.

[0120] 8. Antibacterial performance test

[0121] According to the improved experimental method in AATCC 100-2004 "Antimicrobial Finish on Textile Materials: Evaluation", the antibacterial properties of the samples were tested. Gram-negative Escherichia coli O157:H7 (ATCC 43895) and Gram-positive Staphylococcus aureus (ATCC 6538) were selected as test bacteria, and the fiber membrane was tested for antibacterial properties. The antibacterial rate was calculated according to the following formula: R = (AB) / A × 100%;

[0122] Wherein: R-inhibition rate; A-average colony count of the test sample before treatment; B-average colony count of the test sample after treatment; each group was tested three times and the results were taken as the average value.

[0123] The test results are shown in Table 1 and Table 2.

[0124] Table 1

[0125]

[0126]

[0127] Table 2

[0128]

[0129] like Figure 1 As shown, the surface of the modified polylactic acid fiber in the polylactic acid fiber filtration membrane of the present invention presents a wrinkled structure, with a large specific surface area, and Cu-MOF is well loaded in the wrinkles on the surface of the modified polylactic acid fiber and is not easy to fall off. Figure 2 As shown in Figure 2, the Cu-MOF crystals synthesized by microwave-assisted hydrothermal synthesis have good structural regularity and crystallinity. Figure 3 and Figure 4 As shown, the fiber surfaces of the polylactic acid fiber filtration membranes of Comparative Examples 1 and 2 are smooth, and after the filtration performance test, a large amount of particulate matter is loaded on the membrane surface.

[0130] According to Table 1 and Table 2, the polylactic acid fiber filter membrane of the embodiment has a higher specific surface area, increases the roughness of the fiber, and effectively improves the filtration performance of the fiber membrane. It also has a high surface potential and hardly decays over time, indicating that it has extremely high long-term stability and a long service life. 0.3 and PM 2.5 The filtration efficiency of the examples is above 98%, and the air resistance is much lower than that of the comparative examples, achieving high efficiency and low resistance. Among them, the surface potential of Example 4 is the highest, and it performs best in filtration performance, PM 0.3 and PM 2.5 The filtration efficiency of the samples reached 98.9% and 99.9%, respectively, which is much higher than that of the comparative example 1 (PM 0.3 and PM 2.5 The filtration efficiency is <90%). The antibacterial rate of the polylactic acid fiber filter membrane in the embodiment is as high as 95% or more, which shows good antibacterial performance. The water contact angle of the polylactic acid fiber filter membrane in the embodiment at a time of 10s is all above 120 degrees, which is higher than that of comparative example 1 (water contact angle of 80 degrees) and comparative example 2 (water contact angle of 85 degrees), indicating that the polylactic acid fiber filter membrane of the present invention has good hydrophobicity.

[0131] In summary, the polylactic acid fiber filter membrane provided by the present invention has good surface activity and size uniformity, and has the advantages of high specific surface area, high surface potential, excellent filtration performance, significant antibacterial effect, low air resistance, and long service life.

[0132] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A polylactic acid fiber filter membrane, characterized in that: The polylactic acid fiber filtration membrane comprises modified polylactic acid fibers, the surface of the modified polylactic acid fibers is wrinkled, and the modified polylactic acid fibers comprise a polylactic acid fiber matrix and a MOF material loaded on the surface and inside of the polylactic acid fiber matrix.

2. The polylactic acid fiber filtration membrane according to claim 1, characterized in that: The mass ratio of the polylactic acid fiber matrix to the MOF material is (3-10):1; and / or the average particle size of the MOF material is 100-500 nm; and / or the MOF material includes at least one of a copper-based MOF material and a silver-based MOF material.

3. The polylactic acid fiber filtration membrane according to claim 1, characterized in that: The diameter of the modified polylactic acid fiber is 30-240 nm, and the average pore size is 50-300 nm; and / or the thickness of the polylactic acid fiber filter membrane is 18-350 μm; and / or the specific surface area of ​​the polylactic acid fiber filter membrane is 132-470 m 2 / g; and / or, the water contact angle of the polylactic acid fiber filter membrane is ≥120°.

4. The polylactic acid fiber filtration membrane according to claim 1, characterized in that: At 25°C and 45% humidity, the surface potential of the polylactic acid fiber filter membrane is 7-10 kV; and / or the polylactic acid fiber filter membrane has a surface potential of 7-10 kV for PM 0.3 and PM 2.5 The filtration efficiency is ≥97%; and / or, at a gas flow rate of 10 to 85 L / min, the air resistance of the polylactic acid fiber filter membrane is ≤120 Pa; and / or, at an optical density of 10 to 100 mW / cm 2 Under the condition of high temperature, the antibacterial rate of the polylactic acid fiber filter membrane against Escherichia coli and Staphylococcus aureus is ≥95%.

5. A method for preparing a polylactic acid fiber filtration membrane according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step S1, mixing MOF material, polylactic acid, a template agent and an organic solvent to obtain a spinning solution; Step S2, electrospinning the spinning solution to obtain a fiber membrane precursor; Step S3, soaking the fiber membrane precursor in water to remove the template agent to obtain the polylactic acid fiber filtration membrane.

6. The preparation method according to claim 5, characterized in that: The mass ratio of the MOF material, the polylactic acid, and the template is 1:(3-10):(2-8); Preferably, the mass fraction of the MOF material in the spinning solution is 0.1% to 2%; Preferably, the mass fraction of the polylactic acid in the spinning solution is 0.5% to 10%; Preferably, the mass fraction of the template agent in the spinning solution is 10% to 30%.

7. The preparation method according to claim 5, characterized in that: The organic solvent includes at least one of dichloromethane, chloroform, dimethylformamide, N-methylpyrrolidone, hexafluoroisopropanol, methanol, ethanol, isopropanol, and glycerol; The template is a water-soluble polymer; More preferably, the template comprises at least one of ethylene-vinyl alcohol copolymer, dextran, polyvinyl alcohol, polyacrylamide, and sodium polyacrylate; Preferably, the weight average molecular weight of the polylactic acid is 3×10 4 ~1.5×10 5 .

8. The preparation method according to claim 5, characterized in that: The MOF material includes at least one of a copper-based MOF material and a silver-based MOF material; The preparation method of the copper-based MOF material comprises: The copper salt, trimesic acid and water are mixed, subjected to microwave treatment, and dried to obtain the copper-based MOF material; The preparation method of the silver-based MOF material comprises: Mixing silver salt, 2-methylimidazole and an alcohol solvent, subjecting the mixture to microwave treatment, and drying the mixture to obtain the silver-based MOF material; Preferably, the mass ratio of the trimesic acid to the copper salt is (3-12):1; Preferably, the mass ratio of the 2-methylimidazole to the silver salt is (2-8):1; Preferably, the copper salt includes at least one of copper chloride dihydrate, copper nitrate, and copper acetate; Preferably, the silver salt comprises at least one of silver nitrate, silver fluoride and silver bicarbonate; Preferably, the microwave treatment has a power of 100W to 800W, a temperature of 100 to 180°C, and a time of 1 to 35 minutes.

9. The preparation method according to claim 5, characterized in that: The voltage of the electrostatic spinning is 12 kV to 35 kV, the consumption rate of the spinning solution is 0.6 to 1.2 mL / h, and the receiving distance is 8 to 15 cm.

10. An air filter, characterized in that: The invention comprises the polylactic acid fiber filter membrane described in any one of claims 1 to 4 or the polylactic acid fiber filter membrane prepared by the preparation method described in any one of claims 5 to 9.

Citation Information

Patent Citations

  • Functionalized polyethylenimine-grafted porous nano-fiber adsorption material and preparation thereof

    CN106975465A

  • Ultrathin nano Ag-2MI / PLA (Polylactic Acid) composite electrostatic spinning fiber membrane as well as preparation method and application thereof

    CN114737312A

  • Method for preparing porous polyaniline / polylactic acid conductive fiber

    CN116516520A

  • Composite antibacterial filtering fiber membrane for visually detecting sulfur-containing compounds

    CN117166136A