Manganese-based adsorbent as well as preparation method and application thereof

By using the composite structure of the cationically modified manganese ion sieve and crown ether single-arm resin layer in manganese-based adsorbent, the stability and dissolution problems of manganese-based adsorbent in the process of lithium extraction in the salt lake are solved, and high efficiency and stability are achieved The lithium ion adsorption performance extends the service life.

CN118949946APending Publication Date: 2024-11-15SHENZHEN DIBO ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411144046.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing manganese-based adsorbents have reduced stability and manganese dissolution problems during the lithium extraction process of salt lakes, resulting in reduced intercalation efficiency of lithium ions and reduced adsorption capacity. The dissolution of manganese during acid treatment will damage the structure and shorten the service life.

Method used

The composite structure of the cationically modified manganese ion sieve and the crown ether single-arm resin layer is adopted to improve the specific surface area and structural stability of the manganese ion sieve through the crown ether single-arm resin layer, and to hinder the dissolution of manganese ions through the crown ether single-arm resin layer. The surface of the manganese ion sieve is coated to improve the adsorption efficiency and stability of lithium ions.

Benefits of technology

It significantly improves the adsorption capacity and cycle stability of lithium ions, reduces the manganese dissolution rate, extends the service life of the adsorbent, and maintains efficient lithium ion selective adsorption performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949946A_ABST
    Figure CN118949946A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of salt lake lithium extraction, and particularly provides a manganese-based adsorbent and a preparation method and application thereof.The manganese-based adsorbent comprises a cation modified manganese ion sieve and a crown ether single-arm resin layer; the crown ether single-arm resin layer is coated on the surface of the cation modified manganese ion sieve; a cationic modifier used for cationic modification is selected from one or more of Al2O3, Al (OH) 3, MgO and Mg (OH) 2; preferably, the manganese ion sieve is MnO2. 5H2O, and the manganese ion sieve is MnO2. 5H2O. According to the doped manganese ion sieve, due to the introduction of Al and Mg ions, the specific surface area of the manganese ion sieve is increased, the pore structure is changed, and the contact surface with lithium ions is improved due to the change, so that the lithium ions are adsorbed more easily and efficiently, and lithium ions and hydrogen ions can effectively pass through the ether and single-arm resin layer, and divalent manganese ions are hindered; the crown ether single-arm resin layer wrapping the outside can greatly relieve the solution loss phenomenon of manganese in the circulation process for the manganese ion sieve.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of lithium extraction, and in particular relates to a manganese-based adsorbent, a preparation method and an application thereof. Background Art

[0002] Lithium extraction technology from salt lakes has attracted much attention in recent years, especially in the context of the sharp increase in global lithium demand. Salt lake brines are rich in lithium resources, but the concentration of lithium is low and mixed with high concentrations of coexisting ions such as sodium and magnesium, making efficient lithium extraction a major challenge. Among the many lithium extraction technologies, manganese-based adsorbents have been widely studied and applied due to their high selectivity, economy and environmental friendliness.

[0003] The main types of manganese-based adsorbents include layered manganese oxides and spinel manganese oxides.

[0004] Manganese oxides having a spinel structure include LiMn 2 O 4 and Li 1.33 Mn 1.67 O 4 There are two main types, each with a unique structure and lithium extraction mechanism. 2 O 4 It is a typical spinel structure manganese oxide, in which lithium ions are located in the tetrahedral position of the cubic close-packed oxygen framework, while trivalent and tetravalent manganese ions are located in the octahedral position. During the gradual extraction of lithium, manganese ions are oxidized and finally form λ-MnO 2 λ-MnO 2 With the characteristics of empty tetrahedral positions and tetravalent manganese, this structural change provides an effective channel for the extraction of lithium ions, enabling it to efficiently and selectively adsorb lithium ions from salt lake brine. 1.33 Mn 1.67 O 4 Lithium is extracted by lithium ion-proton exchange. 1.33 Mn 1.67 O 4 The lithium ions are replaced by protons to form spinel manganese oxide with lattice protons. The spinel structure has high chemical stability and selective lithium absorption capacity, and can maintain efficient lithium ion adsorption performance in complex salt lake brine systems.

[0005] Layered manganese oxide Li 1.6 Mn 1.6 O 4 It is a particularly promising lithium-selective adsorbent precursor material with a theoretical lithium ion exchange capacity of up to 73.18 mg / g, high chemical stability, and can be converted into orthorhombic LiMnO by heat treatment at appropriate temperatures. 2 The acid-treated Li1.6 Mn 1.6 O 4 Can form MnO 2 0.5H 2 O, the material shows excellent performance in lithium selective adsorption, especially in the ability to adsorb lithium ions from brine, which is significantly better than other adsorbents. 2 0.5H 2 O retains its cubic structure during acid treatment, showing good grain shape and high crystallinity, with good chemical stability and ion exchange properties. 1.33 Mn 1.67 O 4 Derived MnO 2 0.31H 2 Compared with MnO 2 0.5H 2 O has better crystallinity and higher proton content, which makes it show more superior performance in lithium ion screening and adsorption.

[0006] Patent CN202410249799.1 uses metal ion doping modification to stabilize the crystal structure to improve the performance and service life of the adsorbent. In addition, the process of wet ball milling and spray drying is used to ensure that the raw materials are mixed evenly, and the prepared adsorbent has a moderate particle size, which is suitable for industrial applications. The adsorption capacity of the adsorbent is up to 9.7 mg / g, and the single cycle dissolution rate is about 0.1%.

[0007] Patent CN202410182138.1 first uses phosphoric acid organic compounds to react with vinyl compounds to obtain ionic liquid monomers; secondly, a silane coupling agent containing vinyl is used to modify the manganese-based ion sieve material; finally, the vinyl-modified adsorbent is mixed with the ionic liquid monomer, cross-linking agent, and initiator for polymerization to obtain a lithium ion sieve adsorbent. This method can significantly increase the adsorption capacity of lithium, reduce the dissolution rate of manganese, and improve the stability and service life of the adsorbent. And the process is simple and easy to apply industrially. The adsorption capacity of the adsorbent is as high as 41.5 mg / g, the dissolution rate of a single cycle is 0.08%, and the dissolution rate of 20 cycles is 94.8%.

[0008] Although the above-mentioned manganese-based adsorbents have shown excellent performance in the field of lithium extraction from salt lakes, they also have significant disadvantages, mainly including the following two points:

[0009] (I) Stability problem: Due to Mn 3+ The induced Jahn-Teller effect causes the severe distortion of the octahedral MnO structure, which leads to the decrease of the stability of the Mn-based adsorbent and the reduction of the lithium ion embedding efficiency.

[0010] (ii) Acid treatment dissolution: The dissolution of manganese is particularly obvious during the acid treatment process. This dissolution will not only destroy the adsorbent structure, reduce its adsorption capacity and life, but also weaken its mechanical strength and stability, shortening its service life. Summary of the invention

[0011] The present application proposes a manganese-based adsorbent, comprising a cation-modified manganese ion sieve and a crown ether single-arm resin layer;

[0012] The crown ether single-arm resin layer is coated on the surface of the cation-modified manganese ion sieve;

[0013] The cationic modification agent used in the cationic modification is selected from Al 2 O 3 、Al(OH) 3 、MgO、Mg(OH) 2 One or more of;

[0014] The manganese ion sieve is preferably MnO2·0.5H2O.

[0015] Furthermore, the crown ether single-arm resin is an acrylate crown ether polymer composed of repeating structural units of acrylate crown ether, with a number average molecular weight of 6700 to 15000, wherein m is the number of repetitions of ethoxy groups in the crown ether ring, n is the number of repetitions of acrylate crown ether, and R 1 , R 2 It is the linking group on the enoate crown ether.

[0016] Furthermore, the mass ratio of the cation-modified manganese ion sieve to the crown ether single-arm resin layer is 3-5:8-12.

[0017] Another aspect of the present application provides a method for preparing a manganese-based adsorbent, comprising:

[0018] Preparation of cation-modified manganese ion sieves based on aluminum and magnesium cation modifiers;

[0019] Preparation of crown ether single-arm resin based on 2-hydroxymethyl-crown ether monomer;

[0020] The crown ether single-arm resin, the cation-modified manganese ion sieve, N,N-dimethylformamide, and a surfactant are mixed in a molar ratio of (3-5):(8-12):(8-10):(1-2) to obtain a manganese-based adsorbent.

[0021] Furthermore, the step of preparing the cation-modified manganese ion sieve comprises:

[0022] Dissolve Mn(NO3)2·4H2O in deionized water;

[0023] Place 3-10 times of LiOH·H2O into Mn(NO 3 ) 2 ·In 4H2O solution;

[0024] Add 4-8 times of H2O2 dropwise into the above solution, stir and age to obtain a gel;

[0025] heating the gel at 100-200° C. for 12-48 hours and filtering to obtain LiMnO2 oxide;

[0026] LiMnO2 is preheated and ground with a cationic modifier, and then heated and cooled to obtain a cation-modified manganese ion sieve precursor Li 1.6 Mn 1.6 O4;

[0027] The Li 1.6 Mn 1.6 O4 is added to the HCl solution and filtered to obtain the cation-modified manganese ion sieve MnO2·0.5H2O.

[0028] Furthermore, the cationic modifier is selected from Al 2 O 3 、Al(OH) 3 、MgO、Mg(OH) 2 One or more of .

[0029] Furthermore, the step of preparing the crown ether single-arm resin comprises:

[0030] Mixing 2-hydroxymethyl-crown ether monomer and anhydrous ethanol to obtain a first mixed solution;

[0031] Sodium carbonate is added to the first mixed solution, and then the acyl chloride is added dropwise to the first mixed solution, the reaction temperature is -40°C-60°C, the reaction time is 0.5-12h, and after the reaction is completed, the product is separated by chromatography to obtain a colorless liquid, wherein the molar ratio of the 2-hydroxymethyl-crown ether monomer, anhydrous ethanol, sodium carbonate, and acyl chloride is: 1:4:2:2-6;

[0032] Mixing the colorless liquid with 2-4 times of anhydrous ethanol to obtain a second mixed solution;

[0033] Under a saturated nitrogen atmosphere, anhydrous ethanol and 0.1%-2% molar ratio of initiator are mixed and incorporated into the second mixed solution, the reaction temperature is 20°C-100°C, the polymerization time is 2-24h, and after the reaction is completed, the reduced pressure is evaporated and the solid product is washed to obtain the crown ether single-arm resin.

[0034] Furthermore, the 2-hydroxymethyl-crown ether monomer is one or more of 2-hydroxymethyl-12-crown ether-4, 2-hydroxymethyl-15-crown ether-5, and 2-hydroxymethyl-18-crown ether-6, preferably 2-hydroxymethyl-12-crown ether-4.

[0035] Furthermore, the acyl chloride is one or more of acryloyl chloride, methacryloyl chloride, crotonoyl chloride, 3,3-dimethylacryloyl chloride, and 2-fluoroacryloyl chloride, preferably methacryloyl chloride and 2-fluoroacryloyl chloride.

[0036] Furthermore, the initiator is one or more of dicumyl peroxide, azobisisobutyronitrile, potassium persulfate, and hydrogen peroxide, and the preferred initiators are potassium persulfate and dicumyl peroxide.

[0037] Furthermore, the surfactant is selected from one or more of sodium alkylbenzene sulfonate, sodium lauryl sulfate, polyethylene glycol, polysorbate, and lauryl alcohol polyoxyethylene ether, preferably sodium alkylbenzene sulfonate.

[0038] Another aspect of the present application provides an application of a manganese-based adsorbent to extract lithium from salt lake brine, the application comprising:

[0039] The manganese-based adsorbent in any of the above technical solutions and the manganese-based adsorbent obtained by the preparation method in any of the above technical solutions are applied to the process of extracting lithium from salt lake brine to obtain lithium material.

[0040] One aspect of the present application provides a lithium adsorbent for extracting lithium from salt lake brine, comprising: a manganese-based adsorbent in any of the above technical solutions, or a manganese-based adsorbent obtained by the preparation method in any of the above technical solutions.

[0041] The above technical solution of the present application has at least the following beneficial technical effects:

[0042] (1) Due to the introduction of Al and Mg ions, the specific surface area of ​​the doped manganese ion sieve increases and the pore structure changes. This change increases the contact area with lithium ions, making the adsorption of lithium ions easier and more efficient.

[0043] (2) The crown ether single-arm resin layer can effectively pass lithium ions and hydrogen ions, but block divalent manganese ions. The crown ether single-arm resin layer coated on the outside can greatly alleviate the dissolution of manganese during the circulation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the conventional technology, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0045] Figure 1 is the XRD of the manganese ion sieve LMO and SMO in one embodiment of the present application;

[0046] Figure 2 It is the FT-IR of the manganese ion sieve LMO and SMO in one embodiment of the present application;

[0047] Figure 3 It is a manganese-based adsorbent SEM in one embodiment of the present application. DETAILED DESCRIPTION

[0048] To make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the embodiments of the present application will be described in detail below in conjunction with the accompanying drawings. However, it will be appreciated by those skilled in the art that in the embodiments of the present application, many technical details are proposed in order to enable the reader to better understand the present application. However, even without these technical details and various changes and modifications based on the following embodiments, the technical scheme claimed in the present application can also be implemented. The division of the following embodiments is for the convenience of description, and the specific implementation of the present application should not be construed as any limitation, and the various embodiments can be combined with each other and quoted from each other without contradiction.

[0049] The manganese-based adsorbent in the prior art has the problems of high dissolution rate and low stability.

[0050] The stability problem of manganese-based adsorbents and the dissolution problem of manganese can be attributed to the redox reaction of the crystals. Under acidic conditions, the trivalent manganese (Mn 3+ ) undergoes a redox reaction and is converted into tetravalent manganese (Mn 4+ ) and divalent manganese (Mn 2+ ), where divalent manganese is easily dissolved into the solution, resulting in a reduction in the manganese content in the adsorbent, i.e., a high dissolution rate. In addition, the dissolution of manganese can also pollute the environment. If the dissolved manganese ions are not effectively treated, they may pollute water and soil, increasing treatment costs and complexity.

[0051] To solve the above problems, an embodiment of the present application provides a manganese-based adsorbent for lithium extraction, which includes a cation-modified manganese ion sieve and a crown ether single-arm resin layer coated on the outer surface of the cation-modified manganese ion sieve, and is a composite manganese-based adsorbent.

[0052] The cationic modifier is selected from Al 2 O 3 、Al(OH) 3 、MgO、Mg(OH) 2 One or more of; preferably Al 2 O 3 The manganese ion sieve is preferably MnO2·0.5H2O. The mass ratio of the cation-modified manganese ion sieve to the crown ether single-arm resin layer is 3-5:8-12.

[0053] It should be noted that the manganese ion sieve or manganese ion sieve precursor (such as Li 1.6 Mn 1.6 The principle of lithium ion adsorption by manganese oxide (MnO4) is based on the insertion / deinsertion conversion of lithium ions in the crystal structure of manganese oxide. The lithium ions in manganese oxide are replaced by other cations (such as H + ) is replaced by acid treatment in an acidic solution. 1.6 Mn 1.6 O 4 After acid treatment, lithium ions are exchanged for protons to form manganese oxides containing protons (such as MnO 2 0.5H 2 O). The protons of the proton-containing manganese oxide can be exchanged with lithium ions under specific conditions (for example, using 2 mol / L hydrochloric acid) to restore its lithium ion adsorption capacity.

[0054] This application doped aluminum and magnesium ions into Li 1.6 Mn 1.6 O 4 In the structure of 3+ / ). Since the ion radius of Al and Mg is similar to that of Mn and the bond energy with oxygen is large, the stability of the lattice structure is enhanced after doping, which can reduce the lattice collapse of the lithium ion sieve during the adsorption and desorption process; at the same time, due to the introduction of Al and Mg ions, the specific surface area of ​​the manganese ion sieve after doping increases and the pore structure changes. This change increases the contact surface with lithium ions, making the adsorption of lithium ions easier and more efficient.

[0055] The crown ether single-arm resin is an acrylate crown ether polymer composed of repeating structural units of acrylate crown ether, with a number average molecular weight of 6700 to 15000, where m is the number of repetitions of ethoxy groups in the crown ether ring, n is the number of repetitions of acrylate crown ether, and R 1 , R 2 It is the linking group on the enoate crown ether.

[0056] The repetition number m of the ethoxy group in the crown ether ring includes m=1, 2 and 3, that is, the acrylate crown ether includes acrylate 12 crown 4, acrylate 15 crown 5 and acrylate 18 crown 6. Preferably, the repetition number m of the ethoxy group in the acrylate crown ether ring is 1, that is, the acrylate crown ether is acrylate 12 crown 4, and the diameter of its crown ether ring cavity is equivalent to the diameter of lithium ions. In addition, due to the strengthening effect of the ester group, it has specific adaptability to lithium ions and significantly improves its selective separation ability.

[0057] Linking group R on enoate crown ether 1 Including CH 3 -, F, H, R 2 Including CH 3 -, H, preferably R 1 =CH 3 - or F, or R 2 =CH 3 -, that is, the acrylate in the acrylate crown ether is an acrylate derivative with rigid groups such as methyl, fluoride ion, etc. The rigid groups are connected to the main chain of the acrylate crown ether polymer, which significantly improves the rigidity of the main chain, thereby improving the ability of the acrylate crown ether polymer to capture lithium ions.

[0058] A layer of crown ether single-arm resin shell is wrapped on the outer surface of the manganese ion sieve. The crown ether single-arm resin itself has lithium adsorption sites and a suitable hole structure, which gives the crown ether single-arm resin an intrinsic specific selection ability, so that it can only pass ions of a certain size. During the adsorption and desorption process of the manganese ion sieve, the crown ether single-arm resin layer can effectively pass lithium ions and hydrogen ions, but block divalent manganese ions. From the perspective of Gibbs free energy theory and entropy theory, it can be considered that under acidic conditions, trivalent manganese (Mn 3+ ) undergoes a redox reaction and is converted into tetravalent manganese (Mn 4+ ) and divalent manganese (Mn 2+ ) process will no longer proceed in the forward direction, thereby cutting off the dissolution of manganese. Therefore, the crown ether single-arm resin layer coated on the outside can greatly alleviate the dissolution of manganese in the circulation process for the manganese ion sieve.

[0059] Another aspect of the present application provides a method for preparing a manganese-based adsorbent, which can be used to prepare the manganese-based adsorbent for lithium extraction in any of the above technical solutions. The preparation method specifically includes:

[0060] S1. Preparation of crown ether single-arm resin based on 2-hydroxymethyl-crown ether monomer;

[0061] S2. Preparation of cation-modified manganese ion sieves based on aluminum and magnesium cation modifiers.

[0062] S3. Crown ether single-arm resin, cation-modified manganese ion sieve, N,N-dimethylformamide (DMF), and surfactant are mixed in a molar ratio of (3-5):(8-12):(8-10):(1-2) to obtain a primary mixed solution; wherein DMF is used as a solvent, which swells the crown ether single-arm resin, and the crown ether single-arm resin structure becomes loose before mixing, and the manganese ion sieve is coated after mixing. The swelling effect of the polymer crown ether single-arm resin on water is completely different from that on the solvent (DMF), so the penetration of some manganese ions can be further blocked during the adsorption / desorption of lithium ions.

[0063] S4. dropping the primary mixed solution into deionized water and ethanol to form a millimeter-scale spherical complex with a particle size of generally 1-10 um;

[0064] S5. The spherical complex is washed; then dried at a drying temperature of 80 ° C. The drying is vacuum dried at a vacuum degree of 0.05;

[0065] S6. Use dilute hydrochloric acid to elute to obtain a manganese-based adsorbent. The concentration of dilute hydrochloric acid is about 0.5 mol / L. The purpose of elution is to wash away N,N-dimethylformamide and surfactants. Since manganese ion sieves and crown ether single-arm resins are coordinated with hydrogen ions when removing lithium, dilute hydrochloric acid is used instead of pure water for elution.

[0066] In some embodiments of the present application, the step of preparing the crown ether single-arm resin in step S1 comprises:

[0067] S11. A mixed solution of 0.2 mol of 2-hydroxymethyl-crown ether monomer and 4 times of anhydrous ethanol (ETHO) was placed in a two-necked flask stirred by a magnetic rotor to obtain a first mixed solution;

[0068] S12. Add 2 times of sodium carbonate to the first mixed solution, and then add 2-6 times of the acid chloride dropwise to the first mixed solution. The reaction temperature is -40℃-60℃, and the reaction time is 0.5-12h. After the reaction is completed, the product is separated by chromatography column chromatography to obtain a colorless liquid, wherein the molar ratio of 2-hydroxymethyl-crown ether monomer, anhydrous ethanol, sodium carbonate, and acid chloride is: 1:4:2:2-6; wherein sodium carbonate is an esterification auxiliary agent, and can also be sodium hydroxide, ammonia water or triethylamine.

[0069] S13. 0.1 mol of colorless liquid and 4 times of anhydrous ethanol were mixed in two flasks stirred by a magnetic rotor to obtain a second mixed solution;

[0070] S14. Under a saturated nitrogen atmosphere, anhydrous ethanol and 0.1%-2% molar ratio of initiator are mixed and added into the second mixed solution, the reaction temperature is 20℃-100℃, the polymerization time is 2-24h, and after the reaction is completed, the reduced pressure is evaporated and the solid product is washed to obtain a crown ether single-arm resin.

[0071] In some embodiments of the present application, the 2-hydroxymethyl-crown ether monomer is one or more of 2-hydroxymethyl-12-crown ether-4, 2-hydroxymethyl-15-crown ether-5, 2-hydroxymethyl-18-crown ether-6, preferably 2-hydroxymethyl-12-crown ether-4.

[0072] In some embodiments of the present application, the acyl chloride is one or more of acryloyl chloride, methacryloyl chloride, crotonoyl chloride, 3,3-dimethylacryloyl chloride, and 2-fluoroacryloyl chloride, preferably methacryloyl chloride and 2-fluoroacryloyl chloride.

[0073] In some embodiments of the present application, the initiator is one or more of dicumyl peroxide, azobisisobutyronitrile, potassium persulfate, and hydrogen peroxide, and the preferred initiators are potassium persulfate and dicumyl peroxide.

[0074] In some embodiments of the present application, the step S2 of preparing the cation-modified manganese ion sieve specifically includes:

[0075] S21. Dissolve Mn(NO3)2·4H2O in deionized water; add 3-10 times of LiOH·H2O under vigorous stirring to obtain a third mixed solution;

[0076] S22. Add 4-8 times of H2O2 dropwise into the third mixed solution, stir and age to obtain a black gel. Generally, continue stirring for 1-10 hours and then age for 0.5-5 hours.

[0077] S23. The gel is transferred to a reactor, heated at 100-200 ° C for 12-48 hours, then filtered, washed, precipitated, and dried at 60 ° C to obtain LiMnO2 (LMO);

[0078] S24. After preheating LiMnO2 in air at 300°C for 2 hours, the mixture was fully ground with a cationic modifier for 45 min, wherein the molar ratio of LiMnO2 to the cationic modifier was 1:1%-10%;

[0079] After uniform mixing, the mixture is heated in air at 400-700°C for 4-12 hours, and then cooled to obtain the cation-modified manganese ion sieve precursor Li 1.6 Mn 1.6 O4;

[0080] S25. Cation-modified manganese ion sieve precursor Li 1.6 Mn 1.6 O4 was added to the HCl solution, stirred for 24 hours, filtered, washed, and dried to obtain the cation-modified manganese ion sieve MnO2·0.5H2O (SMO). Figure 1The XRD of manganese ion sieve LMO and SMO is shown. XRD is used to measure the crystal form of manganese ion sieve. The horizontal and vertical axes of XRD are angles and the vertical axis is the measured peak intensity without units. Figure 2 It is the FT-IR of the manganese ion sieve LMO and SMO in one embodiment of the present application. FT-IR is Fourier infrared spectroscopy used to measure the structure of the manganese ion sieve.

[0081] In some embodiments of the present application, the surfactant is selected from one or more of sodium alkylbenzene sulfonate, sodium lauryl sulfate, polyethylene glycol, polysorbate, and lauryl alcohol polyoxyethylene ether; the preferred surfactant is sodium alkylbenzene sulfonate.

[0082] In the aforementioned technical scheme, the preparation of the crown ether single-arm resin in step S1 and the preparation of the cation-modified manganese ion sieve in step S2 are performed separately and in no particular order, and the synthesis of the manganese-based adsorbent is performed after both are prepared. Different from this, in other technical schemes, the cation-modified manganese ion sieve is prepared first, and the raw materials for preparing the crown ether single-arm resin are also prepared, and then the manganese ion sieve is coated during the polymer polymerization process of the crown ether single-arm resin, followed by elution and other processes, and finally the manganese-based adsorbent is obtained. Figure 3 This is a scanning electron microscope (SEM) image of the composite manganese-based adsorbent.

[0083] The following specific examples are further explanations of the present application. The examples cited cannot list all implementation methods of the present application. Only some of them are used as examples for explanation. The specific examples are as follows:

[0084] Example 1

[0085] (1) Preparation of manganese ion sieve:

[0086] 0.1 mol of Mn(NO 3 ) 2 ·4H 2 O was dissolved in 500 mL of deionized water; under vigorous stirring, 4 times (0.4 mol) of LiOH·H 2 O to obtain the third mixed solution. Add 5 times (0.5 mol) H 2 O 2 Add dropwise into the obtained third mixed solution, stir for 2 hours, and age for 2 hours to obtain a black gel.

[0087] The black gel was transferred to a stainless steel autoclave lined with polytetrafluoroethylene (PTFE) and heated at 150°C for 24 hours. The precipitate was filtered, washed, and dried at 60°C to obtain LiMnO 2 The oxide (LMO) was preheated in air at 300℃ for 2 hours to 2 With 5% Al 2 O3 Grind thoroughly for 45 minutes, heat in air at 500°C for 8 hours, and cool to obtain <h2 style=";text-align:left;direction:ltr">Al / Li<h2 style=";text-align:left;direction:ltr"> 1.6 <h2 style=";text-align:left;direction:ltr"> Mn<h2 style=";text-align:left;direction:ltr"> 1.6 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 4 <h2 style=";text-align:left;direction:ltr"> (Al / LMO) .

[0088] 2 g of Al / LMO was added to 120 mL of 0.5 mol / L HCl solution, stirred for 24 hours, filtered, washed, and dried at 60 °C to obtain cation-modified manganese ion sieve MnO. 2 0.5H 2 O(Al / SMO).

[0089] (2) Preparation of crown ether single-arm resin:

[0090] 0.2 mol of 2-hydroxymethyl-15-crown ether-5 and 800 mL of EtOH were used to prepare a first mixed solution. 2 times (0.4 mol) of sodium carbonate was added to the first mixed solution, and 3 times (0.6 mol) of methacryloyl chloride was slowly added dropwise at a reaction temperature of -20°C for 3 hours.

[0091] The product was separated by chromatography to obtain a colorless liquid. 0.1 mol of the colorless liquid was mixed with 400 mL of EtOH, and 0.5% (0.5 mol%) potassium persulfate was added under a saturated nitrogen atmosphere, and the reaction was carried out at 50°C for 12 hours. The product was evaporated under reduced pressure and repeatedly washed to obtain a crown ether single-arm resin.

[0092] (3) Synthetic manganese-based adsorbent:

[0093] Crown ether single-arm resin, cation-modified manganese ion sieve MnO2·0.5H2O, DMF and sodium alkylbenzene sulfonate were mixed in a weight ratio of 3:8:10:1. The mixture was dropped into deionized water and ethanol to form a spherical shape. After washing and drying at 80°C, the mixture was eluted with 0.5 mol / L HCl solution to obtain a millimeter-scale manganese-based adsorbent.

[0094] Example 2

[0095] (1) Preparation of manganese ion sieve:

[0096] Dissolve 0.1 mol of Mn(NO3)2·4H2O in 600 mL of deionized water. Under vigorous stirring, add 5 times (0.5 mol) of LiOH·H2O to obtain a third mixed solution. Add 6 times (0.6 mol) of H2O2 dropwise to the obtained third mixed solution, stir for 3 hours, and age for 3 hours to obtain a black gel. Transfer the gel to a stainless steel high-pressure reactor lined with PTFE and heat at 160°C for 36 hours. Filter and wash the precipitate, and dry it at 60°C to obtain MnO2 oxide (MO). Preheat in air at 320°C for 2 hours, fully grind MO with 3% Al(OH)3 in a molar ratio for 45 minutes, heat in air at 600°C for 10 hours, and obtain Al / Li after cooling.1.6 Mn 1.6 4 g of Al / LMO was added to 80 mL of 0.5 mol / L HCl solution, stirred for 24 hours, filtered, washed, and dried at 60°C to obtain the cation-modified manganese ion sieve MnO2·0.5H2O (Al / SMO).

[0097] (2) Preparation of crown ether single-arm resin

[0098] 0.2 mol of 2-hydroxymethyl-18-crown-6 and 800 mL of EtOH were prepared into a first mixed solution. 2 times (0.4 mol) of sodium carbonate was added to the first mixed solution, and 4 times (0.8 mol) of crotonyl chloride was slowly added dropwise, the reaction temperature was -10 ° C, and the reaction was performed for 6 hours. The product was separated by chromatographic column chromatography to obtain a colorless liquid. 0.1 mol of the colorless liquid was mixed with 400 mL of EtOH, and 1% (1 mol%) of diisopropylbenzene peroxide was added under a saturated nitrogen atmosphere, and the reaction was performed at 30 ° C for 24 hours. The product was evaporated under reduced pressure and repeatedly rinsed to obtain a crown ether single-arm resin.

[0099] (3) Synthesis of manganese-based adsorbent

[0100] Crown ether single-arm resin, cation-modified manganese ion sieve MnO2·0.5H2O, DMF and sodium lauryl sulfate were mixed in a weight ratio of 5:10:10:2, dropped into deionized water and ethanol to form a sphere, washed, dried at 80°C, and eluted with 0.5 mol / L HCl solution to obtain a manganese-based adsorbent.

[0101] Example 3

[0102] (1) Preparation of manganese ion sieve

[0103] Dissolve 0.1 mol of Mn(NO3)2·4H2O in 700 mL of deionized water.

[0104] Under vigorous stirring, add 6 times (0.6 mol) of LiOH·H2O to obtain a third mixed solution. Add 7 times (0.7 mol) of H2O2 dropwise to the third mixed solution, stir for 4 hours, and age for 4 hours to obtain a black gel. Transfer the gel to a stainless steel high-pressure reactor lined with PTFE and heat at 180°C for 48 hours. Filter and wash the precipitate, and dry it at 60°C to obtain MnO2 oxide (MO). Preheat in air at 350°C for 2 hours, fully grind MO with MgO with a molar ratio of 4% for 45 minutes, heat in air at 700°C for 12 hours, and cool to obtain Mg / Li 1.6 Mn 1.6O4 (Mg / LMO). 6 g of Mg / LMO was added to 120 mL of 0.5 mol / L HCl solution, stirred for 24 hours, filtered, washed, and dried at 60°C to obtain a cation-modified manganese ion sieve MnO2·0.5H2O (Mg / SMO).

[0105] (2) Preparation of crown ether single-arm resin

[0106] 0.2 mol of 2-hydroxymethyl-12-crown ether-4 and 800 mL of EtOH were used to prepare a first mixed solution. 2 times (0.4 mol) of sodium carbonate was added to the first mixed solution, and 5 times (1 mol) of 3,3-dimethylacryloyl chloride was slowly added dropwise. The reaction temperature was 0°C and the reaction was carried out for 8 hours. The product was separated by chromatographic column chromatography to obtain a colorless liquid. 0.1 mol of the colorless liquid was mixed with 400 mL of EtOH, and 2% (2 mol%) of azobisisobutyronitrile was added under a saturated nitrogen atmosphere, and the reaction was carried out at 40°C for 18 hours. The product was evaporated under reduced pressure and repeatedly rinsed to obtain a crown ether single-arm resin.

[0107] (3) Synthesis of manganese-based adsorbent

[0108] Crown ether single-arm resin, cation-modified manganese ion sieve MnO2·0.5H2O, DMF and polyethylene glycol were mixed in a weight ratio of 3:10:8:1, dropped into deionized water and ethanol to form a sphere, washed, dried at 80°C, and eluted with 0.5 mol / L HCl solution to obtain a manganese-based adsorbent.

[0109] Embodiment 4:

[0110] (1) Preparation of manganese ion sieve

[0111] Dissolve 0.1 mol of Mn(NO3)2·4H2O in 700 mL of deionized water. Add 3 times (0.3 mol) of LiOH·H2O under vigorous stirring to obtain a third mixed solution. Add 8 times (0.8 mol) of H2O2 dropwise to the third mixed solution, stir for 1 hour, and age for 1 hour to obtain a black gel.

[0112] The gel was transferred to a stainless steel autoclave lined with PTFE and heated at 170°C for 24 hours. The precipitate was filtered, washed, and dried at 60°C to obtain MnO2 oxide (MO). MO was preheated in air at 300°C for 2 hours, and MO was fully ground with 2% Mg(OH)2 in a molar ratio for 45 minutes, heated in air at 450°C for 6 hours, and cooled to obtain Li 1.6 Mn 1.6O4 (Mg / LMO). 6 g of Mg / LMO was added to 120 mL of 0.5 mol / L HCl solution, stirred for 24 hours, filtered, washed, and dried at 60°C to obtain the manganese ion sieve MnO2·0.5H2O (Mg / SMO).

[0113] (2) Preparation of crown ether single-arm resin

[0114] 0.2 mol of 2-hydroxymethyl-18-crown ether-6 and 800 mL of EtOH were prepared into a first mixed solution. 2 times (0.4 mol) of sodium carbonate was added to the first mixed solution, and 3 times (0.6 mol) of 2-fluoroacryloyl chloride was slowly added dropwise, the reaction temperature was -30°C, and the reaction was carried out for 4 hours. The product was separated by chromatographic column chromatography to obtain a colorless liquid. 0.1 mol of the colorless liquid was mixed with 400 mL of EtOH, and 0.2% (0.2 mol%) of potassium persulfate was added under a saturated nitrogen atmosphere, and the reaction was carried out at 30°C for 20 hours. The product was evaporated under reduced pressure and repeatedly rinsed to obtain a crown ether single-arm resin.

[0115] (3) Synthesis of manganese-based adsorbent

[0116] Crown ether single-arm resin, manganese ion sieve MnO2·0.5H2O, DMF and polysorbate were mixed in a weight ratio of 4:12:10:1, dropped into deionized water and ethanol to form a sphere, washed, dried at 80°C, and eluted with 0.5 mol / L HCl solution to obtain a manganese-based adsorbent.

[0117] Embodiment 5:

[0118] (1) Preparation of manganese ion sieve

[0119] 0.1 mol of Mn(NO3)2·4H2O was dissolved in 800 mL of deionized water. Under vigorous stirring, 8 times (0.8 mol) of LiOH·H2O was added to obtain a third mixed solution. 4 times (0.4 mol) of H2O2 was added dropwise to the third mixed solution, stirred for 5 hours, and aged for 5 hours to obtain a black gel.

[0120] The gel was transferred to a stainless steel autoclave lined with PTFE and heated at 200°C for 12 hours. The precipitate was filtered, washed, and dried at 60°C to obtain MnO2 oxide (MO). MO was preheated in air at 330°C for 2 hours, and the molar ratio of MO and Al2O3 was fully ground for 45 minutes, heated in air at 650°C for 4 hours, and Al / Li was obtained after cooling. 1.6 Mn 1.6O4 (Al / LMO). 4 g Al / LMO was added to 80 mL 0.5 mol / L HCl solution, stirred for 24 hours, filtered, washed, and dried at 60°C to obtain the manganese ion sieve MnO2·0.5H2O (Al / SMO).

[0121] (2) Preparation of crown ether single-arm resin

[0122] 0.2 mol of 2-hydroxymethyl-12-crown ether-4 and 800 mL of EtOH were prepared into a first mixed solution. 2 times (0.4 mol) of sodium carbonate was added to the first solution, and 4 times (0.8 mol) of crotonyl chloride was slowly added dropwise, the reaction temperature was -10°C, and the reaction was performed for 12 hours. The product was separated by chromatography using a chromatographic column to obtain a colorless liquid. 0.1 mol of the colorless liquid was mixed with 400 mL of EtOH, and 0.5% (0.5 mol%) of azobisisobutyronitrile was added under a saturated nitrogen atmosphere, and the reaction was performed at 40°C for 12 hours. The product was evaporated under reduced pressure and repeatedly rinsed to obtain a crown ether single-arm resin.

[0123] (3) Synthesis of manganese-based adsorbent

[0124] Crown ether single-arm resin, manganese ion sieve MnO2·0.5H2O, DMF and polyethylene glycol were mixed in a weight ratio of 5:10:10:1, dropped into deionized water and ethanol to form a sphere, washed, dried at 80°C, and eluted with 0.5 mol / L HCl solution to obtain a manganese-based adsorbent.

[0125] Comparative Example 1:

[0126] Only manganese-based ion sieve materials were prepared without related composite modification. 0.1 mol of Mn(NO3)2·4H2O was dissolved in 750 mL of deionized water. Under vigorous stirring, 6 times (0.6 mol) of LiOH·H2O were added dropwise. 6 times (0.6 mol) of H2O2 were added dropwise to the solution, stirred for 2 hours, and aged for 3 hours to obtain a black gel. The gel was transferred to a stainless steel high-pressure reactor lined with PTFE and heated at 180°C for 36 hours. The precipitate was filtered, washed, and dried at 60°C to obtain MnO2 oxide (MO). Preheat in air at 320°C for 2 hours and mix MO with 3% Al in a molar ratio. 2 O 3 Grind thoroughly for 45 minutes, heat in air at 600℃ for 10 hours, and cool to obtain Al / Li 1.6 Mn 1.6 O4.

[0127] 4 g Al / LMO was added to 80 mL 0.5 mol / L HCl solution, stirred for 24 hours, filtered, washed, and dried at 60 °C to obtain manganese ion sieve MnO2·0.5H2O (Al / SMO)

[0128] Test methods and standards:

[0129] (1) Adsorption capacity test: Simulated salt lake brine: Na + 99.32g / L, Mg 2+ 16.8g / L, Li + 0.79g / L, Cl - 198.4g / L, K + 16.7g / L, SO 4 2- 21.1g / L, pH value is 7.32.

[0130] The adsorbent material (the adsorbent obtained in the embodiment and the comparative example) was placed in a group of simulated salt lake brine (pre-adsorption solution) respectively, and stirred and adsorbed at a temperature of 15°C, a stirring speed of 300r / min, and an adsorption time of 2h. After adsorption, vacuum filtration was performed to obtain a post-adsorption solution and a loaded adsorbent material. The loaded adsorbent material was taken and desorbed with a hydrochloric acid solution having a concentration of 1mol / L at a speed of 300r / min and a desorption time of 2h. After desorption, vacuum filtration was performed to obtain a desorbed solution and an unloaded adsorbent material. The element concentrations in the pre-adsorption solution, the post-adsorption solution, and the desorption solution were determined by ICP-MS.

[0131] The adsorption capacity of the adsorbent material for lithium ions is calculated according to the following formula:

[0132] Qt=(C 0 -C t )×V / m

[0133] Among them, Q t ——Adsorption capacity, C 0 ——Lithium ion concentration of solution before adsorption, C t ——Lithium ion concentration of the solution after adsorption, V——volume of the solution, m——mass of the adsorption material.

[0134] (2) Manganese dissolution test: The lithium ion sieve adsorbent particles were washed with HCl at a solid-liquid ratio of 1:100 at room temperature for 24 hours, and the supernatant was taken out with a pipette. The metal cation concentration in the solution was measured using ICP-OES, and then the manganese dissolution rate (DEMn) was calculated. The calculation formula is as follows:

[0135] 1-DEMn=1-(C1×V1) / m,

[0136] Wherein, C1 (mg / L) is the detected concentration of manganese ions, V1 (L) is the volume of the solution, and m (g) is the mass of the adsorbent powder.

[0137] The manganese-based adsorbents prepared in Examples 1 to 5 and Comparative Example 1 were used to perform a simulation test on lithium extraction from a salt lake. The test results are shown in Table 1 below.

[0138] Table 1 Performance results of adsorbents obtained in Examples and Comparative Examples

[0139]

[0140] According to the comparison of the experimental data of the above-mentioned five embodiments of the present application and the comparative example, it can be seen that the cation-modified manganese-based adsorbent coated with a crown ether single-arm resin layer prepared by the method of the present application, compared with the manganese-based ion sieve material in the prior art, has a very significantly reduced single-cycle dissolution rate while ensuring a significant improvement in the lithium ion adsorption capacity, and the dissolution rate for multiple cycles is also very stably maintained at a very low level, which proves that the modified manganese-based adsorbent of the present application has a lower dissolution rate and cycle stability.

[0141] Due to the limitation of pore size, the high molecular crown ether single-arm resin layer of the manganese-based adsorbent can only pass ions with small radius such as lithium and hydrogen, and hinder the seepage of manganese ions; in this application, the cation-modified manganese ion sieve and the crown ether single-arm resin layer combine inorganic and organic groups, which can screen and adsorb lithium ions, not only inhibiting manganese seepage, but also not affecting the adsorption amount of the overall adsorbent during coating, and the prepared adsorbent has strong comprehensive performance. It can be seen from the parameters of the relevant embodiments tested in the above table that the manganese-based adsorbents in Examples 1-5 maintain excellent adsorption capacity during the lithium extraction process of salt lakes, and have low dissolution rate and cycle stability.

[0142] Another aspect of the present application provides an application of a manganese-based adsorbent to extract lithium from salt lake brine, the application comprising:

[0143] The manganese-based adsorbent in any of the above technical solutions and the manganese-based adsorbent obtained by the preparation method in any of the above technical solutions are applied to the process of extracting lithium from salt lake brine to obtain lithium material.

[0144] One aspect of the present application provides a lithium adsorbent for extracting lithium from salt lake brine, comprising: a manganese-based adsorbent in any of the above technical solutions, or a manganese-based adsorbent obtained by the preparation method in any of the above technical solutions.

[0145] In summary, this application provides a manganese-based composite adsorbent for lithium extraction from salt lakes, and its preparation method and application are intended to solve the stability and dissolution problems faced by manganese-based adsorbents in the process of lithium extraction from salt lakes. 1.6 Mn 1.6 O 4 ) as the base material and by doping Al 2 O 3, MgO and other cationic modifiers to improve the structural stability of the material and reduce the dissolution of manganese. At the same time, the specific selectivity of the crown ether single-arm resin is utilized to further enhance the selective adsorption effect of the adsorbent on lithium ions, and significantly inhibit the dissolution process of manganese ions. The technical scheme of the present application achieves efficient and stable lithium ion adsorption performance by optimizing the synthesis process conditions, doping modification and surface protection measures. The experimental results show that the manganese-based composite adsorbent exhibits excellent adsorption capacity and cycle stability in the process of lithium extraction from salt lakes, and has broad industrial application prospects.

[0146] It should be understood that the above specific embodiments of the present application are only used to illustrate or explain the principles of the present application, and do not constitute a limitation to the present application. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present application should be included in the protection scope of the present application. In addition, the claims attached to the present application are intended to cover all changes and modifications that fall within the scope and boundaries of the attached claims, or the equivalent forms of such scope and boundaries.

Claims

1. A manganese-based adsorbent, characterized in that: It includes a cation-modified manganese ion sieve and a crown ether single-arm resin layer; The crown ether single-arm resin layer is coated on the surface of the cation-modified manganese ion sieve; The cationic modification agent used in the cationic modification is selected from one or more of Al2O3, Al(OH)3, MgO, and Mg(OH)2; The manganese ion sieve is preferably MnO2·0.5H2O.

2. The manganese-based adsorbent according to claim 1, characterized in that The crown ether single-arm resin is an acrylate crown ether polymer composed of the following repeating structural units: acrylate crown ether, and has a number average molecular weight of 6700 to 15000. Wherein, m is the number of repetitions of ethoxy groups in the crown ether ring, n is the number of repetitions of the enoate crown ether, and R1 and R2 are linking groups on the enoate crown ether.

3. The manganese-based adsorbent according to claim 1, characterized in that The mass ratio of the cation-modified manganese ion sieve to the crown ether single-arm resin layer is 3-5:8-12.

4. A method for preparing a manganese-based adsorbent, comprising: Preparation of cation-modified manganese ion sieves based on aluminum and magnesium cation modifiers; Preparation of crown ether single-arm resin based on 2-hydroxymethyl-crown ether monomer; The crown ether single-arm resin, the cation-modified manganese ion sieve, N,N-dimethylformamide, and a surfactant are mixed in a molar ratio of (3-5):(8-12):(8-10):(1-2) to obtain a manganese-based adsorbent.

5. The preparation method according to claim 4, characterized in that: The step of preparing the cation-modified manganese ion sieve comprises: Dissolve Mn(NO3)2·4H2O in deionized water; Place 3-10 times of LiOH·H2O into the Mn(NO3)2·4H2O solution; Add 4-8 times of H2O2 dropwise into the above solution, stir and age to obtain a gel; heating the gel at 100-200° C. for 12-48 hours and filtering to obtain LiMnO2 oxide; LiMnO2 is preheated and ground with a cationic modifier, and then heated and cooled to obtain a cation-modified manganese ion sieve precursor Li 1.6 Mn 1.6 O4; The Li 1.6 Mn 1.6 O4 is added to the HCl solution and filtered to obtain the cation-modified manganese ion sieve MnO2·0.5H2O.

6. The preparation method according to claim 5, characterized in that: The cationic modifier is selected from one or more of Al2O3, Al(OH)3, MgO, and Mg(OH)2.

7. The preparation method according to any one of claims 4 to 6, characterized in that: The step of preparing the crown ether single-arm resin comprises: Mixing 2-hydroxymethyl-crown ether monomer and anhydrous ethanol to obtain a first mixed solution; Sodium carbonate is added to the first mixed solution, and then the acyl chloride is added dropwise to the first mixed solution, the reaction temperature is -40°C-60°C, the reaction time is 0.5-12h, and after the reaction is completed, the product is separated by chromatography to obtain a colorless liquid, wherein the molar ratio of the 2-hydroxymethyl-crown ether monomer, anhydrous ethanol, sodium carbonate, and acyl chloride is: 1:4:2:2-6; Mixing the colorless liquid with 2-4 times of anhydrous ethanol to obtain a second mixed solution; Under a saturated nitrogen atmosphere, anhydrous ethanol and 0.1%-2% molar ratio of initiator are mixed and incorporated into the second mixed solution, the reaction temperature is 20°C-100°C, the polymerization time is 2-24h, and after the reaction is completed, the reduced pressure is evaporated and the solid product is washed to obtain the crown ether single-arm resin.

8. The preparation method according to any one of claims 4 to 7, characterized in that: The 2-hydroxymethyl-crown ether monomer is one or more of 2-hydroxymethyl-12-crown ether-4, 2-hydroxymethyl-15-crown ether-5, and 2-hydroxymethyl-18-crown ether-6, preferably 2-hydroxymethyl-12-crown ether-4.

9. The preparation method according to any one of claims 7-8, characterized in that: The acyl chloride is one or more of acryloyl chloride, methacryloyl chloride, crotonoyl chloride, 3,3-dimethylacryloyl chloride, and 2-fluoroacryloyl chloride, preferably methacryloyl chloride and 2-fluoroacryloyl chloride.

10. The preparation method according to any one of claims 7-8, characterized in that: The initiator is one or more of dicumyl peroxide, azobisisobutyronitrile, potassium persulfate, and hydrogen peroxide, and the preferred initiators are potassium persulfate and dicumyl peroxide.

11. The preparation method according to any one of claims 4 to 10, characterized in that: The surfactant is selected from one or more of sodium alkylbenzene sulfonate, sodium lauryl sulfate, polyethylene glycol, polysorbate, and lauryl alcohol polyoxyethylene ether, preferably sodium alkylbenzene sulfonate.

12. An application of a manganese-based adsorbent to extract lithium from salt lake brine, characterized in that: The applications include: The manganese-based adsorbent described in any one of claims 1 to 3 and the manganese-based adsorbent obtained by the preparation method described in any one of claims 4 to 11 are applied to the process of extracting lithium from salt lake brine to obtain lithium material.

13. A lithium adsorbent for extracting lithium from salt lake brine, characterized in that: include: The manganese-based adsorbent according to any one of claims 1 to 3, or the manganese-based adsorbent obtained by the preparation method according to any one of claims 4 to 11.