Method for efficiently recovering zinc from low-grade copper-lead-zinc ore

Through flotation technology and multiple selection sweep technology, the problem of low zinc recovery efficiency in low-grade copper-lead zinc ore is solved, and efficient recycling of zinc concentrate is achieved, simplified the process flow and improved the utilization efficiency of natural resources.

CN118950234APending Publication Date: 2024-11-15LIANGSHAN MINING CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411137339.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing low-grade copper lead-zinc ore processing process is complex, there are many agents and may contain toxic substances, resulting in low zinc recycling efficiency and difficulty in handling tailings, making it difficult to effectively recover natural resources.

Method used

The flotation process is combined with magnetic separation and multiple selection sweeps. By adding an appropriate amount of inhibitor, collector and activator, zinc minerals are isolated and enriched, the process is simplified and the grade and recovery of zinc concentrate are improved.

Benefits of technology

It has achieved efficient recycling of zinc concentrate, with a grade greater than 48.08% and a recovery rate greater than 62.14%, simplifying the process flow and reducing the loss of natural resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950234A_ABST
    Figure CN118950234A_ABST
Patent Text Reader

Abstract

The invention provides a method for efficiently recovering zinc from low-grade copper-lead-zinc ore, which comprises the following steps of: grinding raw ore, roughing by a magnetic separator to obtain rough concentrate, grinding the rough concentrate, then carrying out magnetic separation and concentration to obtain sulfur concentrate, adding an inhibitor and a collecting agent into the magnetic separation roughing tailings in a flotation machine, carrying out lead roughing, and recovering the zinc from the copper-lead-zinc ore. After an activating agent and a collecting agent are added into the lead roughing tailings in a flotation machine, zinc concentrate is obtained through twice refining and twice sweeping; the flotation process is good in zinc recovery effect, high in zinc concentrate recovery rate and significant to recycling of natural resources; and after zinc flotation, zinc concentrate with the grade larger than 48.08% and the recovery rate larger than 62.14% is obtained through two times of concentration and two times of sweeping.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymetallic ore dressing, and in particular to a method for efficiently recovering zinc from low-grade copper-lead-zinc ore. Background Art

[0002] Lead and zinc metals needed in the fields of machinery, chemical industry, military and medicine mainly come from sulfide lead-zinc ores. In lead-zinc ores, not only lead and zinc coexist closely, but also copper, silver, sulfur, iron and other elements are often irregularly intercalated and coexist. Under the general trend of increasingly poor, fine and mixed mineral resources, a reasonable and effective mineral processing process is an important means of recycling natural resources. Copper, lead and zinc ores are often intercalated with each other, and various types of gangue coexist with them in a complex manner. After being fully dissociated by grinding, a reasonable mineral processing system is used to recover various valuable minerals separately, and products with the highest grade and recovery rate as possible are obtained, which can effectively protect natural resources and reduce metal loss. An effective mineral processing system has become the focus of research in the industry. The existing process is long, the reagents are complex, the process is cumbersome, and it is possible to add highly toxic reagents, resulting in problems such as difficult handling of tailings and recovery in the later stage. Therefore, it is very necessary to develop a method that can solve the above technical problems. Summary of the invention

[0003] The purpose of the present invention is to provide a method for efficiently recovering zinc from low-grade copper-lead-zinc ore, which has a short flotation process, good zinc recovery effect, high zinc concentrate recovery rate, and is of great significance to the recycling of natural resources. After zinc flotation, two refinements and two sweeps are performed to obtain a zinc concentrate with a grade greater than 48.08% and a recovery rate greater than 62.14%.

[0004] The embodiments of the present invention are implemented by the following technical solutions:

[0005] A method for efficiently recovering zinc from low-grade copper-lead-zinc ore comprises the following steps:

[0006] S1. Pretreatment: The raw ore of low-grade copper, lead and zinc ore is crushed and ground, and then subjected to magnetic separation to obtain coarse magnetic separation b and coarse magnetic separation tailings c; the coarse magnetic separation b is ground and magnetically separated to obtain sulfur concentrate and magnetic separation tailings d; it should be noted that the main metal minerals in the ore are pyrrhotite, sphalerite, galena, chalcopyrite, pyrite, marcasite, magnetite, hematite, etc.; pyrrhotite and magnetite are mainly separated in the magnetic separation section;

[0007] S2. Lead flotation: mainly concentrate galena and chalcopyrite into lead concentrate

[0008] S21. The coarse magnetic tailings c and the magnetic tailings d are mixed and then an inhibitor and a collector are added to obtain a flotation ore e and a flotation tailings f;

[0009] S22. The flotation ore e is subjected to a primary concentration to obtain a lead concentrate and a middling ore 1;

[0010] S23. The flotation tailings f are added with a collector and subjected to a scavenging process to obtain the middlings 2 and the lead flotation tailings g;

[0011] S3. Zinc flotation: mainly enriched with sphalerite

[0012] S31. The lead flotation tailings g are added with an activator and a collector for zinc flotation to obtain flotation ore h and flotation tailings i;

[0013] S32. The flotation ore h is subjected to two concentrations to obtain zinc concentrate, middlings 3 and middlings 4;

[0014] S33. Add an activator and a collector to the flotation tailings i, and obtain tailings and middlings 5 ​​and 6 after two scavenging operations; the tailings mainly contain pyrite, marcasite, hematite, etc.

[0015] Further, S1 includes the following steps:

[0016] S11. The raw ore is ball-milled to a content of 70% of -0.074 mm, and the slurry is obtained after slurry adjustment, and then the slurry is fully stirred for standby use;

[0017] S12. Add fully stirred ore pulp into the magnetic separator at a uniform speed, and perform rough separation at a magnetic field strength of 2000oe to obtain coarse magnetic concentrate b and coarse magnetic tailings c. Grind the coarse magnetic concentrate b to -0.074, accounting for 80%, and then add it to the magnetic separation equipment, and separate it at a magnetic field strength of 2000oe to obtain sulfur concentrate and magnetically selected tailings d.

[0018] Further, in S21, the inhibitor is any one or more of sodium sulfide, zinc sulfate, and sodium sulfite, the collector is any one or more of No. 25 black medicine, No. 31 black medicine, aniline black medicine, and butylamine black medicine, the added amount of the inhibitor is 1000-1200g / t (the total amount of coarse magnetic separation tailings c and magnetic concentration tailings d), and the added amount of the collector is 50-70g / t (the total amount of coarse magnetic separation tailings c and magnetic concentration tailings d).

[0019] Further, in S31, the activator is any one or more of copper sulfate, oxalic acid, and citric acid, the collector is any one or more of butyl xanthate, isobutyl xanthate, pentyl xanthate, and isopentyl xanthate, the added amount of the activator is 300-400g / t (total amount of lead flotation tailings in g), and the added amount of the collector is 300-400g / t (total amount of lead flotation tailings in g).

[0020] Furthermore, in S32, during the first concentration, a primary concentration reagent is added, wherein the primary concentration reagent comprises, by mass percentage, 50% to 70% of butyrrolidone and 30% to 50% of dithiocarbamate; in an environment of divalent copper ions activated by an activator such as copper sulfate, the primary concentration reagent acts on the surface of the sphalerite to form hydrophobic bonds, and the rising bubbles in the flotation machine are separated from the ore pulp to achieve the enrichment of the sphalerite. During the second concentration, a secondary concentration reagent is added, which includes sodium isobutyl xanthate, sodium naphthalene sulfonate, copper sulfate and pine oil in a mass ratio of 5-8:3-4:1-2:1; during flotation, sodium isobutyl xanthate and sodium naphthalene sulfonate form competitive adsorption on the surface of carbonaceous materials (such as graphite), which can reduce its consumption of sodium isobutyl xanthate and ensure the flotation recovery of the target mineral; and sodium naphthalene sulfonate can inhibit the adsorption of sodium isobutyl xanthate in the pulp by carbonaceous materials, thereby ensuring that more sodium isobutyl xanthate reacts with lead, zinc and sulfur minerals to ensure its flotation recovery effect.

[0021] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:

[0022] The flotation process of the present invention has the advantages of short process flow, good zinc recovery effect and high recovery rate of zinc concentrate, and is of great significance to the recovery and utilization of natural resources. After zinc flotation, two concentrations and two sweeps are performed to obtain zinc concentrate with a grade greater than 48.08% and a recovery rate greater than 62.14%. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0024] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0026] Example 1

[0027] This embodiment provides a method for efficiently recovering zinc from low-grade copper-lead-zinc ore, comprising the following steps:

[0028] A. Pretreatment: ball-mill the raw ore to -0.074 mm with a content of 70% to obtain material a;

[0029] B. Magnetic separation desulfurization:

[0030] 1) Add material a into a magnetic separator, and separate the material b and tailings c at a field strength of 2000oe;

[0031] 2) Grind the coarse magnetic ore b to -0.074 accounting for 80% and then add it into the magnetic separator to separate the sulfur concentrate and magnetic tailings d at a field strength of 2000oe;

[0032] C. Lead flotation:

[0033] 1) The coarse magnetic tailings c and the magnetic tailings d are mixed and added into a flotation machine, and 1000 g / t of zinc sulfate and 60 g / t of 25# black medicine are added at the same time, and then flotation is performed to obtain flotation ore e and flotation tailings f;

[0034] 2) flotation ore e is subjected to primary concentration to obtain lead concentrate and middling ore 1;

[0035] 3) Adding a collector to the flotation tailings f and subjecting it to a first sweep to obtain the middlings 2 and the lead flotation tailings g;

[0036] D. Zinc flotation:

[0037] 1) adding 300 g / t of copper sulfate and 80 g / t of butyl xanthate to the lead flotation tailing g to carry out zinc flotation to obtain flotation ore h and flotation tailing i;

[0038] 2) adding 60 g / t of butyl xanthate and 40 g / t of dithiocarbamate to the flotation ore h for the first concentration, and then performing the second concentration, and adding 50 g / t of sodium isobutyl xanthate, 30 g / t of sodium naphthalenesulfonate, 10 g / t of copper sulfate and 10 g / t of pine oil to obtain zinc concentrate, middling ore 3 and middling ore 4;

[0039] 3) The flotation tailing i is scavenged twice with activator copper sulfate and collector butyric acid xanthate, wherein the amount of copper sulfate added in the first scavenging is 150 g / t and the amount of butyric acid xanthate added is 40 g / t, and the amount of copper sulfate added in the second scavenging is 50 g / t and the amount of butyric acid xanthate added is 20 g / t; after scavenging, tailings and middlings 5 ​​and 6 are obtained.

[0040] The treatment method of this embodiment obtains a zinc concentrate with a grade of 49.12% and a recovery rate of 68.14%.

[0041] Example 2

[0042] The difference between this embodiment and embodiment 1 is that: during lead flotation, in step C1), the inhibitor is sodium sulfite, and the addition amount is 600 g / t; the collector is No. 31 black medicine, and the addition amount is 60 g / t; during zinc flotation, in step D2), during the first concentration, 70 g / t of butyl xanthate and 30 g / t of dithiocarbamate are added; during the second concentration, 60 g / t of sodium isobutyl xanthate, 20 g / t of sodium naphthalenesulfonate, 10 g / t of copper sulfate and 10 g / t of pine oil are added.

[0043] The treatment method of this embodiment obtains a zinc concentrate with a grade of 49.08% and a recovery rate of 67.01%.

[0044] Example 3

[0045] The difference between this embodiment and embodiment 1 is that: during lead flotation, in step C1), the inhibitor is sodium sulfite, and the addition amount is 600 g / t; the collector is No. 31 black medicine, and the addition amount is 60 g / t; during zinc flotation, in step D2), during the first concentration, 70 g / t of butyl xanthate and 30 g / t of dithiocarbamate are added; during the second concentration, 60 g / t of sodium isobutyl xanthate, 20 g / t of sodium naphthalenesulfonate, 10 g / t of copper sulfate and 10 g / t of pine oil are added.

[0046] The treatment method of this embodiment obtains a zinc concentrate with a grade of 45.08% and a recovery rate of 66.24%.

[0047] Example 4

[0048] The difference between this embodiment and embodiment 1 is that: during lead flotation, in step C1), the inhibitor is sodium sulfite, and the addition amount is 600 g / t; the collector is No. 31 black medicine, and the addition amount is 60 g / t; during zinc flotation, in step D2), during the first concentration, 70 g / t of butyl xanthate and 30 g / t of dithiocarbamate are added; during the second concentration, 60 g / t of sodium isobutyl xanthate, 20 g / t of sodium naphthalenesulfonate, 10 g / t of copper sulfate and 10 g / t of pine oil are added.

[0049] The treatment method of this embodiment obtains a zinc concentrate with a grade of 46.08% and a recovery rate of 65.77%.

[0050] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for efficiently recovering zinc from low-grade copper-lead-zinc ore, characterized in that: By weight, the method comprises the following steps: S1. Pretreatment: The raw ore of low-grade copper, lead and zinc ore is crushed and ground, and then subjected to magnetic separation to obtain coarse magnetic separation b and coarse magnetic separation tailings c; the coarse magnetic separation b is ground and magnetically separated to obtain sulfur concentrate and magnetic concentration tailings d; S2. Lead flotation: S21. The coarse magnetic tailings c and the magnetic tailings d are mixed and then an inhibitor and a collector are added to obtain a flotation ore e and a flotation tailings f; S22. The flotation ore e is subjected to a primary concentration to obtain a lead concentrate; S23. The flotation tailings f are added with a collector and subjected to a sweep to obtain lead flotation tailings g; S3. Zinc flotation: S31. Adding an activator and a collector to the lead flotation tailings g to carry out zinc flotation to obtain flotation ore h and flotation tailings i; S32. The flotation ore h is subjected to two concentrations to obtain zinc concentrate, middlings 3 and middlings 4; S33. Add an activator and a collector to the flotation tailings i, and obtain tailings and middlings 5 ​​and 6 after two scavenging operations.

2. The method for efficiently recovering zinc from low-grade copper-lead-zinc ore according to claim 1, characterized in that: S1 includes the following steps: S11. The raw ore is ball-milled to a content of 70% of -0.074 mm, and the slurry is obtained after slurry adjustment, and then the slurry is fully stirred for standby use; S12. Add fully stirred ore pulp into the magnetic separator at a uniform speed, and perform rough separation at a magnetic field strength of 2000oe to obtain coarse magnetic concentrate b and coarse magnetic tailings c. Grind the coarse magnetic concentrate b to -0.074, accounting for 80%, and then add it to the magnetic separation equipment, and separate it at a magnetic field strength of 2000oe to obtain sulfur concentrate and magnetically selected tailings d.

3. The method for efficiently recovering zinc from low-grade copper-lead-zinc ore according to claim 1, characterized in that: In S21, the inhibitor is any one or more of zinc sulfate, lime, sodium sulfite, sodium pyrosulfite, calcium hypochlorite, and sodium hypochlorite; and the added amount of the inhibitor is 600-1200 g / t.

4. The method for efficiently recovering zinc from low-grade copper-lead-zinc ore according to claim 1, characterized in that: In S21, the collector is any one or more of No. 25 black medicine, No. 31 black medicine, aniline black medicine, and butylamine black medicine; the added amount of the collector is 50-70g / t.

5. The method for efficiently recovering zinc from low-grade copper-lead-zinc ore according to claim 1, characterized in that: In S31, the activator is any one or more of copper sulfate, oxalic acid, and citric acid, and the added amount of the activator is 300-400g / t.

6. The method for efficiently recovering zinc from low-grade copper-lead-zinc ore according to claim 1, characterized in that: In S31, the collector is any one or more of butyl xanthate, isobutyl xanthate, pentyl xanthate, and isopentyl xanthate, and the added amount of the collector is 300-400 g / t.

7. The method for efficiently recovering zinc from low-grade copper-lead-zinc ore according to claim 1, characterized in that: In S32, during the first concentration, a primary concentration agent is added, wherein the primary concentration agent comprises 50% to 70% of butyrrolidone and 30% to 50% of dithiocarbamate by mass percentage.

8. The method for efficiently recovering zinc from low-grade copper-lead-zinc ore according to claim 1, characterized in that: In S32, during the second concentration, a secondary concentration agent is added, and the secondary concentration agent includes sodium isobutyl xanthate, sodium naphthalenesulfonate, copper sulfate and pine oil in a mass ratio of 4-6:2-3:1-2:1.