Method for preparing multi-performance suspension material under assistance of electric pulse
Through electrical pulse assisted heating technology, local heating is applied during the rolling process of composite sheets, the oxidation problem caused by the overall heating of the elementary sheet is solved, and the preparation of high-performance composite sheets is realized, which improves the NVH performance and production efficiency of the suspension system.
Patent Information
- Application Number
- CN202411146078.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-20
AI Technical Summary
In the existing hot-rolling process for composite sheets, the overall heating of the base sheets leads to surface oxidation, affecting material performance and production efficiency.
Using electrical pulse assisted heating technology, local heating is performed in the deformation area of the plate, instead of overall heating, and cutting and rolling two plates with different conductivity coefficients are determined, and the contact parts are heated between the rolling mill rolls using electrical pulse heating equipment. Control the temperature gradient and avoid oxidation.
It improves the bonding strength and multiple performance characteristics of composite sheets, such as high strength, lightweight, and fast thermal conductivity, enhances the NVH performance of the suspension system and improves production efficiency.
Smart Images

Figure CN118950701A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of automobile manufacturing, and in particular relates to a method for preparing a multi-performance suspension material with the assistance of electric pulses. Background Art
[0002] With the rapid development of the automobile industry, end customers not only pay attention to the technical characteristics of vehicle configuration, but also pay attention to vehicle technical production process methods. In particular, green production process methods have become the main theme of development, which not only saves human resource costs, but also improves production efficiency. The suspension system, as a device for vibration reduction, limiting and connection between the vehicle powertrain and the frame or body, plays an important role in the impact of the vehicle's NVH performance. However, the homogeneous materials used in the inner and outer jackets of the suspension can no longer meet the needs of high-quality development, and should be developed in the direction of composite materials. Therefore, new preparation process methods for composite materials have become a research focus and hotspot.
[0003] like Figure 1 The figure shows a common hot rolling process of composite plates, which is composed of a heating device 01, a base plate 02, and a rolling mill 03. During operation, the heating device heats the base plate, and after reaching a certain temperature, the plate is sent to the rolling mill to prepare a composite material. In the prior art, the base plate is heated as a whole, and the upper and lower surfaces of the plate need to reach the set temperature before rolling begins. This causes the upper and lower surfaces of the base plate to be easily oxidized when in contact with the air before rolling, and the contact surface performance is affected, which restricts the production efficiency of the composite plate. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing multi-performance suspension materials with the assistance of electric pulses. Under the premise of ensuring the bonding performance of the composite material, local heating is performed in the deformation area of the plate to replace the overall heating, thereby avoiding large-area oxidation of the surface of the elementary plate and improving the bonding performance of the composite plate.
[0005] To achieve the above objectives, this application is implemented through the following technical solutions:
[0006] A method for preparing a multi-performance suspension material with the aid of electric pulses, comprising the following steps:
[0007] S1. Determine the electrical conductivity of the two sheets to be composited;
[0008] S2, the length of the plate with a small conductivity coefficient in the rolling direction during cutting is greater than the length of the plate with a large conductivity coefficient;
[0009] S3, placing the two plates up and down, and introducing one end of the two plates together between the two rolls of the two-roll rolling mill;
[0010] S4. Start the electric pulse assisted heating equipment to heat the contact part of the two plates. The two rollers of the two-roll mill drive the two plates to move forward. When the tail end of the shorter plate passes through the closest point between the two rollers, turn off the two-roll mill and the electric pulse assisted heating equipment.
[0011] Furthermore, an introduction part is provided at the front end of the two plates, and when the introduction part is introduced between the two rollers of the two-roller rolling mill, the electric pulse auxiliary heating device is started.
[0012] Furthermore, after being introduced between the two rolls of the two-roll mill, the two rolls of the two-roll mill stop rotating for a set time, and after the electric pulse assisted heating equipment heats the contact part of the two plates to a set temperature, the two rolls of the two-roll mill continue to rotate.
[0013] Furthermore, the length S of the introduction portion is set according to the time t required for the electric pulse device to start heating until the temperature of the contact portion of the two plates reaches the rolling temperature×the speed v at which the two rollers drive the plates forward.
[0014] Furthermore, the electric pulse assisted heating device includes an electric pulse heating device, a first wire and a second wire, one end of the first wire is connected to the positive pole of the electric pulse heating device, and the other end is connected to the tail end of the plate with a small conductivity coefficient; one end of the second wire is connected to the lower roll of the two rolls of the two-roll rolling mill, and the other end is connected to the negative pole of the electric pulse heating device.
[0015] Furthermore, the first wire is connected to the tail end of the plate with a small conductivity coefficient through a connecting piece.
[0016] Furthermore, the connecting member is a bolt or a clamping member.
[0017] Furthermore, if the connecting member is a bolt, a threaded hole is provided at the tail of the plate with a small conductivity coefficient.
[0018] The beneficial effects of the present invention are:
[0019] In the process of preparing composite plates based on this process method, local heating of the deformation zone bonding tip can be achieved instead of overall heating. The process method that can control the heating temperature can prepare composite plates with higher bonding strength, so that the composite materials have multiple performance characteristics such as high strength, light weight, and fast thermal conductivity, enhance the function of the suspension system, and improve the NVH performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of hot rolling process of composite plate in existing technology.
[0021] Figure 2 It is a schematic diagram of the hot rolling process of the composite plate of the present invention.
[0022] Figure 3 This is the current distribution diagram of the pulse current passing through the deformation zone of the composite plate.
[0023] Figure 4 This is the current change diagram of the deformation zone of the composite plate after the pulse current ends.
[0024] Figure 5 This is the overall distribution diagram of temperature in the composite plate during pulse current heating.
[0025] Figure 6 This is the overall distribution curve of temperature in the composite plate during pulse current heating.
[0026] Figure 7 This is a schematic diagram of the current flow during the pulse current heating process.
[0027] Description of reference numerals:
[0028] 01. Heating equipment; 02. Elementary plate; 03. Rolling mill equipment; 1. Two-roll rolling mill; 2. Composite plate; 3. Second conductor; 4. Pulse auxiliary heating equipment; 5. Bolts; 11. Roller; 21. Copper plate; 22. Aluminum plate. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is described in detail below in conjunction with the accompanying drawings. The following embodiments are merely exemplary and can only be used to explain and illustrate the technical solution of the present invention, but cannot be construed as limiting the technical solution of the present invention.
[0030] like Figure 2 and Figure 7 As shown, the present application relates to a method for preparing multi-performance suspension materials with the assistance of electric pulses. In the present technology, the rolling mill used in the composite plate rolling process is a two-roll rolling mill 1. Because the two-roll rolling mill is a commonly used equipment in the field, the applicant does not explain the structure of the two-roll rolling mill. Technical personnel in the field can choose according to actual needs, and it will not affect the implementation of the technical solution of the present application.
[0031] The improvement focus of this technical solution is the rolling process. The conventional heating equipment used in the original composite rolling is not used, that is, the composite rolling of this application does not heat the entire or large area of the rolled plate. In order to improve the surface oxidation problem of the plate during the composite rolling process, this technical solution uses the electric pulse discharge characteristics and the microscopic sensitivity to metal materials to locally heat the two plates to be composited, forming a temperature gradient change on the surface of the plate.
[0032] The processing technology of this application specifically adopts the following steps:
[0033] S1. Determine the electrical conductivity of the two plates to be composited. Because in actual production, the materials of the two plates to be composited are usually different, and the composite plates of this technical solution are all made of metal, and do not involve the composite of metal plates and other non-metallic plates.
[0034] S2. The length of the plate with a small conductivity coefficient in the rolling direction during cutting is greater than the length of the plate with a large conductivity coefficient. Specifically, the plate with a small conductivity coefficient is placed above the plate with a large conductivity coefficient. In the technical solution of the present application, the composite of the copper plate 21 and the aluminum plate 22 is used as an example for explanation, wherein the conductivity of the copper plate is less than that of the aluminum plate. In this embodiment, the two plates to be composited are both rectangular as an example for explanation, wherein the length of the plate with a small conductivity coefficient is greater than the length of the aluminum plate.
[0035] In other embodiments of the present application, an introduction part is also provided at the front end of the two plates, which is used to introduce the two plates into between the two rollers 11 of the two-roll mill 1. In other embodiments of the present application, because the relative surfaces of the two plates need to be rolled together, and the pulse-assisted heating equipment needs to perform several current pulses to heat the surfaces of the contact points of the two plates to a set temperature, an introduction part is introduced for this purpose. When the introduction parts of the two plates pass through the two rollers of the two-roll mill, the pulse-assisted heating equipment 4 heats the contact points to reach the rolling temperature.
[0036] The length S of the introduction portion is set according to the time t required for the electric pulse assisted heating device to start heating until the temperature of the contact portion of the two plates reaches the rolling temperature×the speed v at which the two rollers 11 drive the plates forward.
[0037] In other embodiments of the present application, the material waste in the rolling process can be reduced by not using the lead-in part, thereby reducing the problem of increased material cost caused by shearing the lead-in part after the composite is completed.
[0038] S3. Place the two plates up and down, and introduce one end of the two plates into between the two rollers 11 of the two-roller rolling mill.
[0039] S4. Start the electric pulse auxiliary heating equipment to heat the contact part of the two plates. The two rollers of the two-roll mill drive the two plates to move forward. When the tail end of the shorter plate passes through the closest point between the two rollers, turn off the two-roll mill and the pulse auxiliary heating equipment 4.
[0040] In other embodiments of the present application, because no introduction part is provided for the two plates, waste of material can be avoided, and after the plates to be compounded are introduced between the two rollers of the two-roll mill, the two rollers of the two-roll mill stop rotating for a set time, and after the pulse-assisted heating device 4 heats the contact part of the two plates to a set temperature, the two rollers 11 of the two-roll mill continue to rotate.
[0041] like Figure 7 As shown, the electric pulse assisted heating device of the present application includes an electric pulse heating device, a first wire and a second wire, one end of the first wire is connected to the positive pole of the electric pulse heating device, and the other end is connected to the tail end of the plate with a small conductivity coefficient; one end of the second wire 3 is connected to the lower roller of the two rollers of the two-roller mill, and the other end is connected to the negative pole of the electric pulse heating device. The first wire is connected to the tail end of the plate with a small conductivity coefficient through a connecting member; wherein the connecting member is one of a bolt or a clamping member. If the connecting member is a bolt 5, a threaded hole is provided at the tail of the plate with a small conductivity coefficient.
[0042] Working principle:
[0043] In the rolling process of composite plates, the deformation bonding area of composite rolling is actually very small, and physical means cannot achieve the expected measurement target. In addition, the pulse discharge duration (pulse width) is only tens of microseconds, which also restricts the implementation of actual observation. Therefore, simulation software is used to illustrate the temperature gradient formation process. The electrothermal coupling pre-treatment method of the deformation zone is adopted. The two plates are connected to square wave pulses with parameters of 365V-500Hz-80μs. When the pulse discharges, the current flows through the deformation zone of the composite plate, and obvious current concentration appears in the bonding zone, forming a disturbance effect. The maximum regional current density is 1.16×1012A / m2, such as Figure 3 At the end of the pulse discharge, the current in the entire composite plate deformation zone disappears, and the variable current effect disappears as well, as shown in Figure 4 As shown. When a certain pulse is applied for a certain time, the temperature of the deformation zone will rise rapidly during discharge in a single cycle, and the temperature will drop immediately when the discharge ends. The temperature drop rate is lower than the rise rate. Under the continuous action of multiple pulse cycles, the temperature of the joint gradually increases. At 0.4s, the maximum temperature of the deformation zone can reach 85.4℃, while the temperature from the entrance to the tail of the composite plate is still at room temperature, forming a temperature gradient, achieving the effect of preheating only the deformation zone, as shown in Figure 5 and Figure 6 shown.
[0044] In order to improve the bonding performance of the composite sheet 2, the temperature of the deformation zone is reasonably controlled by adjusting the voltage, frequency and pulse width of the electric pulse device. In this embodiment, the positive electrode of the pulse power supply is connected to the copper plate, and the pulse current with parameters of 365V-700Hz-70μs flows from the copper plate to the aluminum plate in the common plastic forward sliding zone of the deformation zone, and then the current flows from the aluminum plate to the lower roller of the two rollers of the two-roller rolling mill, and finally flows out to the bearing seats at both ends, and is connected to the negative electrode of the pulse current to form a complete working circuit, such as Figure 7It should be noted that when the rolling is near the end, the rolling mill and pulse power supply are immediately turned off, the copper wire connected by the bolts is manually removed, and the composite plate rolling sample is removed. The maximum temperature of the deformation zone is about 295.5℃ and the peel strength is 6.69N / mm through experimental methods.
[0045] The above describes in detail the structure, features and effects of the present invention based on the embodiments shown in the drawings. The above is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown in the drawings. Any changes made according to the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the description and drawings, should be within the protection scope of the present invention.
Claims
1. A method for preparing a multi-performance suspension material assisted by electric pulses, characterized in that: Use the following steps: S1. Determine the electrical conductivity of the two sheets to be composited; S2, the length of the plate with a small conductivity coefficient in the rolling direction during cutting is greater than the length of the plate with a large conductivity coefficient; S3, placing the two plates up and down, and introducing one end of the two plates together between the two rolls of the two-roll mill; S4. Start the electric pulse auxiliary heating equipment to heat the contact part of the two plates. The two rollers of the two-roll mill drive the two plates to move forward. When the tail end of the shorter plate passes through the closest point between the two rollers, turn off the two-roll mill and the electric pulse auxiliary heating equipment.
2. The method for preparing multi-performance suspension materials with electric pulse assistance according to claim 1, characterized in that: An introduction part is provided at the front end of the two plates. When the introduction part is introduced between the two rolls of the two-roll rolling mill, the electric pulse auxiliary heating device is started.
3. The method for preparing multi-performance suspension materials with electric pulse assistance according to claim 2, characterized in that: The length S of the introduction portion is set based on the time t required for the electric pulse device to start heating until the temperature of the contact portion of the two plates reaches the rolling temperature×the speed v at which the two rollers drive the plates forward.
4. The method for preparing multi-performance suspension materials with electric pulse assistance according to claim 1, characterized in that: After being introduced between the two rolls of the two-roll mill, the two rolls of the two-roll mill stop rotating for a set time, and after the electric pulse auxiliary heating equipment heats the contact part of the two plates to a set temperature, the two rolls of the two-roll mill continue to rotate.
5. The method for preparing multi-performance suspension materials with electric pulse assistance according to claim 1, characterized in that: The electric pulse assisted heating device includes an electric pulse heating device, a first wire and a second wire, one end of the first wire is connected to the positive pole of the electric pulse heating device, and the other end is connected to the tail end of the plate with a small conductivity coefficient; one end of the second wire is connected to the lower roll of the two rolls of the two-roll rolling mill, and the other end is connected to the negative pole of the electric pulse heating device.
6. The method for preparing multi-performance suspension materials with electric pulse assistance according to claim 5, characterized in that: The first conducting wire is connected to the tail end of the plate with a small conductivity through a connecting piece.
7. The method for preparing multi-performance suspension materials with electric pulse assistance according to claim 6, characterized in that: The connecting piece is a bolt or a clamp.
8. The method for preparing multi-performance suspension materials with electric pulse assistance according to claim 7, characterized in that: If the connecting piece is a bolt, a threaded hole is provided at the tail of the plate with a low conductivity coefficient.
Citation Information
Patent Citations
Current assisted vacuum rolling method for preparing metal composite plate
CN108273847A
Pulse current auxiliary rolling method and device for multi-layer metal composite boards
CN108723087A
Method for simultaneously improving strength and plasticity of 2219 aluminum-based AlCoCrFeNi composite material plate
CN112760577A
Pulse current auxiliary wave flat rolling method for high-strength and high-plasticity titanium alloy plate
CN114713628A
Steel / aluminum alloy layered metal composite plate rolling forming method
CN117139371A