Partial instantaneous liquid phase connection method for silicon nitride ceramic / nickel-based superalloy

By using composite brazing filler metal to join silicon nitride ceramics and nickel-based superalloys, adding copper-plated carbon fiber powder to form a sandwich structure and brazing under vacuum conditions, the problem of residual stress caused by differences in thermophysical properties was solved, and the high-temperature strength and stability of the joint were achieved.

CN118951194AActive Publication Date: 2024-11-15HARBIN INST OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411278179.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-15
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

The connection between silicon nitride ceramics and nickel-based superalloys faces the problem of residual stress caused by the large difference in thermophysical properties, resulting in low joint strength.

Method used

A composite brazing method is adopted, which involves adding copper-plated carbon fiber powder to copper-plated titanium powder to control the carbon fiber content in the composite brazing alloy, and then brazing under vacuum conditions to form a sandwich structure of the workpiece to be welded, ensuring the high-temperature performance and strength of the joint.

Benefits of technology

An effective connection between silicon nitride ceramics and nickel-based superalloys was achieved, with no obvious microcracks in the joint, exhibiting good high-temperature mechanical properties and stable strength at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118951194A_ABST
    Figure CN118951194A_ABST
Patent Text Reader

Abstract

The invention discloses a partial instantaneous liquid phase connection method for a silicon nitride ceramic / nickel-based superalloy, and relates to a connection method for the silicon nitride ceramic / nickel-based superalloy. The technical problem that an existing silicon nitride ceramic / nickel-based superalloy connector is low in strength is solved. According to the method, the silicon nitride ceramic-high-temperature nickel-based alloy connector with a good interface is obtained, the composite brazing filler metal is adopted for partial instantaneous liquid phase connection, the high-temperature-resistant connector is obtained, the connector is free of obvious microcracks, thermal expansion of a weld joint is further reduced, and the mechanical property is good. The surface of the carbon fiber powder is subjected to copper coating treatment, the active element Ti in the composite brazing filler metal is prevented from directly reacting with the carbon fiber powder, the reaction of the active element Ti and ceramic is hindered, then a connector with the high carbon fiber volume fraction is obtained, and the highest volume fraction can reach 25%; the obtained joint has no obvious microcracks, and the shear strength at the test high temperature of 800 DEG C can reach 88 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a connection method of silicon nitride ceramics / nickel-based high-temperature alloy. Background Art

[0002] Silicon nitride ceramics have a wide range of practical applications in the aerospace field due to their low thermal expansion coefficient and excellent mechanical properties at high temperatures, but ceramic materials are difficult to process into complex large components. Nickel-based high-temperature alloys (GH4169) have good high-temperature performance and are easy to process and form, but their creep resistance is relatively poor under high-temperature service environments. Therefore, it is of great practical value to prepare silicon nitride ceramics and nickel-based high-temperature alloys into composite components by partial transient liquid phase connection. The biggest problem facing the connection of ceramic-metal dissimilar materials is the residual stress problem caused by the large difference in the thermal physical properties of the parent materials. Reducing the thermal expansion coefficient of the weld by adding low-expansion coefficient particles to the weld is a common method to reduce the residual stress of the joint. By surface modifying the low-expansion carbon fiber powder, increasing the bearing limit of the carbon fiber powder in the weld, effectively increasing the content of carbon fiber in the weld, and reducing the residual stress of the joint, the strength of the joint can be improved. Summary of the invention

[0003] The present invention aims to solve the technical problem of low strength of existing silicon nitride ceramic / nickel-based high-temperature alloy joints and provide a partial instantaneous liquid phase connection method for silicon nitride ceramic / nickel-based high-temperature alloys.

[0004] The partial instantaneous liquid phase bonding method for silicon nitride ceramic / nickel-based high temperature alloy of the present invention is carried out according to the following steps:

[0005] 1. Put the copper-plated carbon fiber powder and the copper-plated titanium powder together in a planetary ball mill, perform low-speed ball milling and mixing, obtain a uniformly mixed composite solder powder, and then prepare a composite solder sheet by the pressure of a tablet press; the volume fraction of the copper-plated carbon fiber powder in the composite solder powder is 5% to 25%;

[0006] 2. Pre-treating the base material nickel-based alloy and the base material silicon nitride ceramic block respectively;

[0007] 3. Placing the composite brazing material sheet in step 1 between the two base materials pre-treated in step 2, and applying adhesive between the layers to obtain a sandwich structure to be welded; in the sandwich structure to be welded, the base material nickel-based alloy is located at the bottom, and the base material silicon nitride ceramic block is located at the top;

[0008] 4. Place the sandwich structure to be welded assembled in step 3 into a vacuum heating furnace, raise the temperature from room temperature to 300℃~310℃ and keep it warm for 30 minutes to ensure that the adhesive is completely volatilized, then raise the temperature to 1000℃~1060℃ and keep it warm for 5min~20min; then lower the temperature to 300℃~310℃, and finally cool naturally to room temperature to complete the brazing process; the entire process of step 4 is carried out under vacuum conditions.

[0009] The present invention aims to obtain a silicon nitride ceramic-high temperature nickel-based alloy joint with a good interface, and adopts a composite solder partial instantaneous liquid phase connection to obtain a high temperature resistant joint, the joint has no obvious microcracks, further reduces the thermal expansion of the weld, and has good mechanical properties. The advantage of the present invention is that it overcomes the disadvantage of limited addition of low expansion coefficient particles in traditional composite solders. The composite solder used in the present invention is obtained by adding copper-plated carbon fiber powder to copper-plated titanium powder to adjust the content of copper-plated carbon fiber in the composite solder; the present invention performs copper coating treatment on the surface of the carbon fiber powder to avoid the active element Ti in the composite solder from directly reacting with the carbon fiber powder, thereby hindering the reaction of the active element Ti with the ceramic, thereby obtaining a connection joint containing a higher volume fraction of carbon fiber, the highest volume fraction of which can reach 25%.

[0010] The process of the invention is simple, and direct brazing of ceramic and metal can be achieved without any modification treatment on the surface of the sample to be welded before welding. Effective connection of ceramic and metal can be achieved by adding composite brazing material. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 This is the assembly drawing of the workpiece to be welded in step 4 of test 1;

[0012] Figure 2 The photos of the joint structure and energy spectrum obtained in Experiment 1;

[0013] Figure 3 This is a photo of the element surface distribution of the joint obtained in Experiment 1. DETAILED DESCRIPTION

[0014] Specific implementation method 1: This implementation method is a partial instantaneous liquid phase connection method for silicon nitride ceramic / nickel-based high-temperature alloy, which is specifically carried out in the following steps:

[0015] 1. Put the copper-plated carbon fiber powder and the copper-plated titanium powder together in a planetary ball mill, perform low-speed ball milling and mixing, obtain a uniformly mixed composite solder powder, and then prepare a composite solder sheet by the pressure of a tablet press; the volume fraction of the copper-plated carbon fiber powder in the composite solder powder is 5% to 25%;

[0016] 2. Pre-treating the base material nickel-based alloy and the base material silicon nitride ceramic block respectively;

[0017] 3. Placing the composite brazing material sheet in step 1 between the two base materials pre-treated in step 2, and applying adhesive between the layers to obtain a sandwich structure to be welded; in the sandwich structure to be welded, the base material nickel-based alloy is located at the bottom, and the base material silicon nitride ceramic block is located at the top;

[0018] 4. Place the sandwich structure to be welded assembled in step 3 into a vacuum heating furnace, raise the temperature from room temperature to 300℃~310℃ and keep it warm for 30 minutes to ensure that the adhesive is completely volatilized, then raise the temperature to 1000℃~1060℃ and keep it warm for 5min~20min; then lower the temperature to 300℃~310℃, and finally cool naturally to room temperature to complete the brazing process; the entire process of step 4 is carried out under vacuum conditions.

[0019] Specific embodiment 2: This embodiment is different from the specific embodiment 1 in that: the preparation method of the copper-plated titanium powder described in step 1 is as follows:

[0020] 1. Soak the pure titanium powder in a mixture of acetone and anhydrous ethanol, perform ultrasonic cleaning for 10 to 15 minutes to remove grease on the surface of the powder, and then filter and dry the powder in sequence at a drying temperature of 70° C. for 30 minutes; the mass proportion of acetone in the mixture of acetone and anhydrous ethanol is 50%; the particle size of the pure titanium powder is 2000 mesh;

[0021] 2. Dissolve SnCl2 in deionized water, then add NaOH and dilute sulfuric acid solution in sequence, then add the powder dried in step 1 and ultrasonically vibrate for 1 min to 3 min, and finally filter and dry in sequence;

[0022] The dilute sulfuric acid solution is 1 mol / L;

[0023] The mass ratio of SnCl2 to deionized water is (1 g to 5 g): 40 mL;

[0024] The mass ratio of SnCl2 to NaOH is 1:(0.4-10);

[0025] The mass ratio of SnCl2 to the volume ratio of the dilute sulfuric acid solution is 1g:(1mL~20mL);

[0026] The mass ratio of the pure titanium powder described in step 1 to the SnCl2 described in step 2 is 1:(0.4-10);

[0027] 3. Mix the silver-based activator and purified water, and then add them to the dried product in step 2. Ultrasonic mixing for 1 to 5 minutes, followed by suction filtration and drying at 70°C for 30 minutes.

[0028] The silver-based activator is a silver ammonia solution with a concentration of 10 g / L;

[0029] The mass ratio of the silver-based activator to pure water is 1:(1-5);

[0030] The volume ratio of the pure titanium powder described in step 1 to the silver-based activator described in step 3 is 1g:(20mL-25mL);

[0031] Fourth, CuSO4.5H2O, potassium sodium tartrate and EDTA-2Na are added to pure water and mixed and stirred, and then NaOH is added to adjust the solution to a pH of 11.5-12.5, and then placed in a water bath at 70°C-75°C, and formaldehyde solution is added dropwise, and then the product dried in step 3 is added, and heated in a water bath at 70°C-75°C for 5min-6min, the solution changes from dark blue to white, and finally filtered and dried in sequence to obtain copper-plated titanium powder, and the thickness of the copper plating layer is 1μm-5μm;

[0032] The mass fraction of the formaldehyde solution is 37%;

[0033] The volume ratio of the formaldehyde solution to pure water is 1:(25-50);

[0034] The mass ratio of potassium sodium tartrate to CuSO4.5H2O is 1:(1.3-1.5);

[0035] The mass ratio of potassium sodium tartrate to EDTA-2Na is 1:(1-1.5);

[0036] The mass ratio of the potassium sodium tartrate to the volume of pure water is 1g:(25mL-30mL);

[0037] The mass ratio of the pure titanium powder in step 1 to the potassium sodium tartrate in step 4 is 1:(6-12). The rest is the same as the first embodiment.

[0038] Specific embodiment 3: This embodiment is different from the specific embodiment 1 in that: the preparation method of the copper-plated carbon fiber powder described in step 1 is as follows:

[0039] 1. Soak the carbon fiber powder in concentrated sulfuric acid, ultrasonically pickle for 10-15 minutes, and then filter and dry in sequence; then ultrasonically clean the pickled and dried carbon fiber powder in deionized water for 10-15 minutes to remove the residual sulfuric acid on the surface of the carbon fiber powder, and then filter and dry in sequence, the drying temperature is 70°C, and the time is 30 minutes; the concentration of the concentrated sulfuric acid is 18.4 mol / L; the carbon fiber powder is a short-diameter carbon fiber of 1000 mesh;

[0040] 2. Dissolve SnCl2 in deionized water, then add NaOH and dilute sulfuric acid solution in sequence, then add the powder dried in step 1 and ultrasonically vibrate for 1 min to 3 min, and finally filter and dry in sequence;

[0041] The dilute sulfuric acid solution is 1 mol / L;

[0042] The mass ratio of SnCl2 to deionized water is (1 g to 5 g): 40 mL;

[0043] The mass ratio of SnCl2 to NaOH is 1:(0.4-10);

[0044] The mass ratio of SnCl2 to the volume ratio of the dilute sulfuric acid solution is 1g:(1mL~20mL);

[0045] The mass ratio of the carbon fiber powder described in step 1 to the SnCl2 described in step 2 is 1:(0.4-10);

[0046] 3. Mix the silver-based activator and purified water, and then add them to the dried product in step 2. Ultrasonic mixing for 1 to 5 minutes, followed by suction filtration and drying at 70°C for 30 minutes.

[0047] The silver-based activator is a silver ammonia solution with a concentration of 10 g / L;

[0048] The mass ratio of the silver-based activator to pure water is 1:(1-5);

[0049] The volume ratio of the carbon fiber powder described in step 1 to the silver-based activator described in step 3 is 1g:(20mL-25mL);

[0050] Fourth, CuSO4.5H2O, potassium sodium tartrate and EDTA-2Na are added to pure water and mixed and stirred, and then NaOH is added to adjust the solution to a pH of 11.5-12.5, and then placed in a water bath at 70°C-75°C, and formaldehyde solution is added dropwise, and then the product dried in step 3 is added, and heated in a water bath at 70°C-75°C for 5min-6min, the solution changes from dark blue to white, and finally filtered and dried in sequence to obtain copper-plated carbon fiber powder, and the thickness of the copper plating layer is 6μm-9μm;

[0051] The mass fraction of the formaldehyde solution is 37%;

[0052] The volume ratio of the formaldehyde solution to pure water is 1:(25-50);

[0053] The mass ratio of potassium sodium tartrate to CuSO4.5H2O is 1:(1.3-1.5);

[0054] The mass ratio of potassium sodium tartrate to EDTA-2Na is 1:(1-1.5);

[0055] The mass ratio of the potassium sodium tartrate to the volume of pure water is 1g:(25mL-30mL);

[0056] The mass ratio of the carbon fiber powder in step 1 to the potassium sodium tartrate in step 4 is 1:(6-12). The rest is the same as the first embodiment.

[0057] Specific implementation method 4: This implementation method is different from the specific implementation method 1 in that the rotation speed of the low-speed ball mill in step 1 is 100 r / min. The rest is the same as the specific implementation method 1.

[0058] Specific embodiment 5: This embodiment differs from specific embodiment 1 in that the pressure of the tablet press in step 1 is 2 MPa. The rest is the same as specific embodiment 1.

[0059] Specific implementation method 6: This implementation method is different from specific implementation method 1 in that: the method for pre-treating the base material nickel-based alloy in step 2 is as follows: the base material nickel-based alloy is treated with water sandpaper to remove the oxide layer and coarse scratches visible to the naked eye on the metal surface, and then polished with 600#, 800#, and 1000# metallographic sandpapers in sequence until there are no obvious scratches on the surface, and finally polished with diamond particles with a particle size of 0.5μm to make the surface to be welded bright; finally, it is ultrasonically cleaned with anhydrous ethanol for 10 minutes and dried for use. Others are the same as specific implementation method 1.

[0060] Specific implementation method 7: This implementation method is different from specific implementation method 6 in that the parent nickel-based alloy is GH4169 nickel-based alloy. Other aspects are the same as specific implementation method 6.

[0061] Specific implementation eight: This implementation is different from specific implementation one in that: the method for pre-treating the base material silicon nitride ceramic block in step two is as follows: the silicon nitride ceramic block is roughly ground on a 400# diamond grinding disc until the sample surface is flat, and then W3.5 diamond grinding paste is used to grind on a flat glass until there is no obvious wire cutting mark on the silicon nitride welding surface, and then W1 grinding paste is used to grind until the silicon nitride ceramic surface is bright, and finally anhydrous ethanol is ultrasonically cleaned for 10 minutes, and dried for use. Others are the same as specific implementation one.

[0062] Specific implementation method 9: This implementation method is different from the specific implementation method 1 in that the adhesive in step 3 is 502 glue. The rest is the same as the specific implementation method 1.

[0063] Specific implementation method 10: This implementation method is different from specific implementation method 1 in that: in step 4, the sandwich structure to be welded assembled in step 3 is placed in a vacuum heating furnace, and the temperature is first raised from room temperature to 300℃~310℃ at a heating rate of 10℃ / min and kept warm for 30min to ensure that the adhesive is completely volatilized, and then the temperature is raised to 1000℃~1060℃ at a heating rate of 10℃ / min and kept warm for 5min~20min; then the temperature is lowered to 300℃~310℃ at a cooling rate of 5℃ / min, and finally naturally cooled to room temperature to complete the brazing process; the entire process of step 4 is carried out under vacuum conditions. Others are the same as specific implementation method 1.

[0064] The present invention is verified by the following tests:

[0065] Test 1: This test is a partial instantaneous liquid phase bonding method for silicon nitride ceramic / nickel-based high-temperature alloy, which is specifically carried out in the following steps:

[0066] 1. Put the copper-plated carbon fiber powder and the copper-plated titanium powder together in a planetary ball mill and mix them by low-speed ball milling at a speed of 100 r / min to obtain a uniformly mixed composite solder powder; take 0.4 mg of the composite solder powder and prepare a composite solder sheet by a tablet press at a pressure of 2 MPa; the volume fraction of the copper-plated carbon fiber powder in the composite solder powder is 20%;

[0067] 2. The base material nickel-based alloy is treated with water sandpaper to remove the oxide layer and the coarse scratches visible to the naked eye on the metal surface, and then polished with 600#, 800#, and 1000# metallographic sandpapers in turn until there are no obvious scratches on the surface, and finally polished with diamond particles with a particle size of 0.5μm to make the surface to be welded bright; finally, ultrasonic cleaning is performed with anhydrous ethanol for 10 minutes, and drying is performed for standby use; the base material nickel-based alloy is GH4169 nickel-based alloy;

[0068] The base material silicon nitride ceramic block was coarsely ground on a 400# diamond grinding disc until the sample surface was flat, and then W3.5 diamond grinding paste was used to grind on a flat glass until there was no obvious wire cutting mark on the silicon nitride welding surface, and then W1 grinding paste was used to grind until the silicon nitride ceramic surface was bright, and finally anhydrous ethanol was ultrasonically cleaned for 10 minutes and dried for use;

[0069] 3. Place the composite solder sheet (the size of the composite solder sheet is slightly larger than the two parent materials) in the middle of the two parent materials pre-treated in step 2, and apply 502 glue between each layer to obtain a sandwich structure to be welded; in the sandwich structure to be welded, the parent material nickel-based alloy is located at the bottom, and the parent material silicon nitride ceramic block is located at the top;

[0070] Fourth, put the sandwich structure to be welded assembled in step 3 into a vacuum heating furnace, first increase the temperature from room temperature to 300℃ at a heating rate of 10℃ / min and keep it warm for 30min to ensure that the 502 glue is completely volatilized, then increase the temperature to 1020℃ at a heating rate of 10℃ / min and keep it warm for 10min; then cool it to 300℃ at a cooling rate of 5℃ / min, and finally cool it naturally to room temperature to complete the brazing process and obtain the joint; the whole process of step 4 is carried out under vacuum conditions, and the vacuum degree should be ensured to be above 1×10 -2 the following.

[0071] The preparation method of the copper-plated titanium powder described in step 1 is as follows:

[0072] 1. Soak the pure titanium powder in a mixture of acetone and anhydrous ethanol, perform ultrasonic cleaning for 10 minutes to remove grease on the surface of the powder, and then filter and dry in sequence at a drying temperature of 70°C for 30 minutes; the mass proportion of acetone in the mixture of acetone and anhydrous ethanol is 50%; the particle size of the pure titanium powder is 2000 mesh;

[0073] 2. Dissolve SnCl2 in deionized water, then add NaOH and dilute sulfuric acid solution in sequence, then add the powder dried in step 1 and ultrasonically vibrate for 3 minutes, and finally filter and dry in sequence;

[0074] The dilute sulfuric acid solution is 1 mol / L;

[0075] The mass ratio of SnCl2 to deionized water is 3g:40mL;

[0076] The mass ratio of SnCl2 to NaOH is 1:5;

[0077] The mass ratio of SnCl2 to the volume ratio of the dilute sulfuric acid solution is 1g:10mL;

[0078] The mass ratio of the pure titanium powder described in step 1 to the SnCl2 described in step 2 is 1:5;

[0079] 3. Mix the silver-based activator and purified water, and then add them to the dried product in step 2. Ultrasonic mixing for 1 minute, followed by suction filtration and drying. The drying temperature is 70°C and the time is 30 minutes.

[0080] The silver-based activator is a silver ammonia solution with a concentration of 10 g / L;

[0081] The mass ratio of the silver-based activator to pure water is 1:4;

[0082] The mass ratio of the pure titanium powder described in step 1 to the volume ratio of the silver-based activator described in step 3 is 1 g:25 mL;

[0083] 4. Add CuSO4.5H2O, sodium potassium tartrate and EDTA-2Na to pure water and mix and stir, then add NaOH to adjust the solution to a pH of 12, then put it in a 75°C water bath, add formaldehyde solution dropwise, then add the dried product in step 3, heat in a 75°C water bath for 6 minutes, the solution changes from dark blue to white, finally filter and dry in sequence to obtain copper-plated titanium powder, the thickness of the copper plating is 3 μm;

[0084] The mass fraction of the formaldehyde solution is 37%;

[0085] The volume ratio of the formaldehyde solution to pure water is 1:30;

[0086] The mass ratio of potassium sodium tartrate to CuSO4.5H2O is 1:1.5;

[0087] The mass ratio of potassium sodium tartrate to EDTA-2Na is 1:1.5;

[0088] The mass ratio of potassium sodium tartrate to pure water is 1g:30mL;

[0089] The mass ratio of the pure titanium powder described in step 1 to the potassium sodium tartrate described in step 4 is 1:10.

[0090] The preparation method of the copper-plated carbon fiber powder described in step 1 is as follows:

[0091] a. Soak the carbon fiber powder in concentrated sulfuric acid, ultrasonically pickle for 10 minutes, and then filter and dry in sequence; then ultrasonically clean the pickled and dried carbon fiber powder in deionized water for 10 minutes to remove the residual sulfuric acid on the surface of the carbon fiber powder, and then filter and dry in sequence, the drying temperature is 70°C, and the time is 30 minutes; the concentration of the concentrated sulfuric acid is 18.4 mol / L; the carbon fiber powder is a short-diameter carbon fiber of 1000 mesh;

[0092] b. Dissolve SnCl2 in deionized water, then add NaOH and dilute sulfuric acid solution in sequence, then add the powder dried in step a and ultrasonically vibrate for 3 minutes, and finally filter and dry in sequence;

[0093] The dilute sulfuric acid solution is 1 mol / L;

[0094] The mass ratio of SnCl2 to deionized water is 3g:40mL;

[0095] The mass ratio of SnCl2 to NaOH is 1:8;

[0096] The mass ratio of SnCl2 to the volume ratio of the dilute sulfuric acid solution is 1g:20mL;

[0097] The mass ratio of the carbon fiber powder described in step a to the SnCl2 described in step b is 1:10;

[0098] c. Mix the silver-based activator and purified water, and then add them to the dried product in step 2. Ultrasonic mixing for 3 minutes is followed by suction filtration and drying. The drying temperature is 70° C. and the time is 30 minutes.

[0099] The silver-based activator is a silver ammonia solution with a concentration of 10 g / L;

[0100] The mass ratio of the silver-based activator to pure water is 1:5;

[0101] The mass ratio of the carbon fiber powder described in step a to the volume ratio of the silver-based activator described in step c is 1 g:25 mL;

[0102] d. Add CuSO4.5H2O, sodium potassium tartrate and EDTA-2Na to pure water, mix and stir, then add NaOH to adjust the solution to a pH of 12, then put it in a 75°C water bath, add formaldehyde solution dropwise, then add the dried product in step c, heat in a 75°C water bath for 6 minutes, the solution changes from dark blue to white, finally filter and dry in sequence to obtain copper-plated carbon fiber powder, the thickness of the copper plating layer is 8 μm;

[0103] The mass fraction of the formaldehyde solution is 37%;

[0104] The volume ratio of the formaldehyde solution to pure water is 1:40;

[0105] The mass ratio of potassium sodium tartrate to CuSO4.5H2O is 1:1.4;

[0106] The mass ratio of potassium sodium tartrate to EDTA-2Na is 1:1.5;

[0107] The mass ratio of potassium sodium tartrate to pure water is 1g:30mL;

[0108] The mass ratio of the carbon fiber powder described in step a to the potassium sodium tartrate described in step d is 1:10.

[0109] Figure 1 This is the assembly diagram of the workpiece to be welded in step 4 of experiment 1, where 1 is the base material Si3N4 ceramic, 2 is the middle layer metal, and 3 is the base material nickel-based high-temperature alloy GH4169.

[0110] After the final step four connection is completed, there is no obvious microcrack in the silicon nitride ceramic / GH4169 alloy joint, the room temperature shear strength of the joint is 97MPa, and the shear strength of the joint at the test high temperature of 800°C is 88MPa.

[0111] Figure 2 The photos of the joint organization and energy spectrum obtained in experiment 1 are shown in Figure b, Figure c, Figure c, Figure c, Figure d, Figure d, Figure d, Figure e, Figure b, Figure a, Figure f, Figure c, Figure g, Figure a. It can be seen from the photos of the joint organization that the joint is well bonded and no obvious defects are found. Combined with the energy spectrum results, it is shown that the main organization of the weld is a copper-based solid solution, in which there is a small amount of dispersed Cu-Ti intermetallic compound phase, a TiC reaction layer around the carbon fiber, and a TiN reaction layer (point C) adjacent to the base material silicon nitride ceramic. During the connection process, the titanium element in the composite solder reacts with silicon nitride to form a TiN layer, the molten solder dissolves the copper plating layer, and reacts with the carbon fiber to form a TiC phase.

[0112] Figure 3 The element surface distribution photos of the joint were obtained for Experiment 1. The surface scanning results showed that in addition to being enriched on the surface of silicon nitride, titanium was also widely present around the carbon fiber particles; the Cr element was also detected to be concentrated around the carbon fiber near the GH4169 side.

[0113] Experiment 2: This experiment is different from Experiment 1 in that:

[0114] The volume fraction of the copper-plated carbon fiber powder in the composite solder powder in step 1 is 10%;

[0115] In step 4, the temperature was raised to 1040°C and kept at this temperature for 5 minutes. The rest was the same as in experiment 1. After the connection in step 4 was completed, there was no obvious microcrack in the silicon nitride ceramic / GH4169 alloy joint, the room temperature shear strength of the joint was 79 MPa, and the shear strength of the joint at the test high temperature of 800°C was 61 MPa.

[0116] Test 3: This test is different from Test 1 in that:

[0117] The volume fraction of the copper-plated carbon fiber powder in the composite solder powder in step 1 is 15%;

[0118] In step 4, the temperature was raised to 1060°C and kept at this temperature for 5 minutes. The rest was the same as in experiment 1. After the connection in step 4 was completed, there was no obvious microcrack in the silicon nitride ceramic / GH4169 alloy joint, the room temperature shear strength of the joint was 83MPa, and the shear strength of the joint at the test high temperature of 800°C was 69MPa.

[0119] Test 4: This test is different from Test 1 in that:

[0120] The volume fraction of the copper-plated carbon fiber powder in the composite solder powder in step 1 is 5%;

[0121] In step 4, the temperature was raised to 1000°C and kept at this temperature for 20 minutes. The rest was the same as in experiment 1. After the connection in step 4 was completed, there was no obvious microcrack in the silicon nitride ceramic / GH4169 alloy joint, and the room temperature shear strength of the joint was 61 MPa.

Claims

1. A partial instantaneous liquid phase bonding method for silicon nitride ceramic / nickel-based high temperature alloy, characterized in that The partial transient liquid phase bonding method for silicon nitride ceramic / nickel-based high temperature alloy is carried out in the following steps:

1. Put the copper-plated carbon fiber powder and the copper-plated titanium powder together in a planetary ball mill, perform low-speed ball milling and mixing, obtain a uniformly mixed composite solder powder, and then prepare a composite solder sheet by the pressure of a tablet press; the volume fraction of the copper-plated carbon fiber powder in the composite solder powder is 5% to 25%; 2. Pre-treating the base material nickel-based alloy and the base material silicon nitride ceramic block respectively; 3. Placing the composite brazing material sheet in step 1 between the two base materials pre-treated in step 2, and applying adhesive between the layers to obtain a sandwich structure to be welded; in the sandwich structure to be welded, the base material nickel-based alloy is located at the bottom, and the base material silicon nitride ceramic block is located at the top; 4. Place the sandwich structure to be welded assembled in step 3 into a vacuum heating furnace, raise the temperature from room temperature to 300℃~310℃ and keep it warm for 30 minutes to ensure that the adhesive is completely volatilized, then raise the temperature to 1000℃~1060℃ and keep it warm for 5min~20min; then lower the temperature to 300℃~310℃, and finally cool naturally to room temperature to complete the brazing process; the entire process of step 4 is carried out under vacuum conditions.

2. A method for partial transient liquid phase bonding of silicon nitride ceramics / nickel-based high-temperature alloys according to claim 1, characterized in that The preparation method of the copper-plated titanium powder described in step 1 is as follows:

1. Soak the pure titanium powder in a mixture of acetone and anhydrous ethanol, perform ultrasonic cleaning for 10 to 15 minutes to remove grease on the surface of the powder, and then filter and dry the powder in sequence at a drying temperature of 70° C. for 30 minutes; the mass proportion of acetone in the mixture of acetone and anhydrous ethanol is 50%; the particle size of the pure titanium powder is 2000 mesh; 2. Dissolve SnCl2 in deionized water, then add NaOH and dilute sulfuric acid solution in sequence, then add the powder dried in step 1 and ultrasonically vibrate for 1 min to 3 min, and finally filter and dry in sequence; The dilute sulfuric acid solution is 1 mol / L; The mass ratio of SnCl2 to deionized water is (1 g to 5 g): 40 mL; The mass ratio of SnCl2 to NaOH is 1:(0.4-10); The mass ratio of SnCl2 to the volume ratio of the dilute sulfuric acid solution is 1g:(1mL~20mL); The mass ratio of the pure titanium powder described in step 1 to the SnCl2 described in step 2 is 1:(0.4-10); 3. Mix the silver-based activator and purified water, and then add them to the dried product in step 2. Ultrasonic mixing for 1 to 5 minutes, followed by suction filtration and drying at 70°C for 30 minutes. The silver-based activator is a silver ammonia solution with a concentration of 10 g / L; The mass ratio of the silver-based activator to pure water is 1:(1-5); The volume ratio of the pure titanium powder described in step 1 to the silver-based activator described in step 3 is 1g:(20mL-25mL); Fourth, CuSO4.5H2O, potassium sodium tartrate and EDTA-2Na are added to pure water and mixed and stirred, and then NaOH is added to adjust the solution to a pH of 11.5-12.5, and then placed in a water bath at 70°C-75°C, and formaldehyde solution is added dropwise, and then the product dried in step 3 is added, and heated in a water bath at 70°C-75°C for 5min-6min, the solution changes from dark blue to white, and finally filtered and dried in sequence to obtain copper-plated titanium powder, and the thickness of the copper plating layer is 1μm-5μm; The mass fraction of the formaldehyde solution is 37%; The volume ratio of the formaldehyde solution to pure water is 1:(25-50); The mass ratio of potassium sodium tartrate to CuSO4.5H2O is 1:(1.3-1.5); The mass ratio of potassium sodium tartrate to EDTA-2Na is 1:(1-1.5); The mass ratio of the potassium sodium tartrate to the volume of pure water is 1g:(25mL-30mL); The mass ratio of the pure titanium powder described in step 1 to the potassium sodium tartrate described in step 4 is 1:(6-12).

3. A method for partial transient liquid phase bonding of silicon nitride ceramics / nickel-based high-temperature alloys according to claim 1, characterized in that The preparation method of the copper-plated carbon fiber powder described in step 1 is as follows:

1. Soak the carbon fiber powder in concentrated sulfuric acid, ultrasonically pickle for 10-15 minutes, and then filter and dry in sequence; then ultrasonically clean the pickled and dried carbon fiber powder in deionized water for 10-15 minutes to remove the residual sulfuric acid on the surface of the carbon fiber powder, and then filter and dry in sequence, the drying temperature is 70°C, and the time is 30 minutes; the concentration of the concentrated sulfuric acid is 18.4 mol / L; the carbon fiber powder is a short-diameter carbon fiber of 1000 mesh; 2. Dissolve SnCl2 in deionized water, then add NaOH and dilute sulfuric acid solution in sequence, then add the powder dried in step 1 and ultrasonically vibrate for 1 min to 3 min, and finally filter and dry in sequence; The dilute sulfuric acid solution is 1 mol / L; The mass ratio of SnCl2 to deionized water is (1 g to 5 g): 40 mL; The mass ratio of SnCl2 to NaOH is 1:(0.4-10); The mass ratio of SnCl2 to the volume ratio of the dilute sulfuric acid solution is 1g:(1mL~20mL); The mass ratio of the carbon fiber powder described in step 1 to the SnCl2 described in step 2 is 1:(0.4-10); 3. Mix the silver-based activator and purified water, and then add them to the dried product in step 2. Ultrasonic mixing for 1 to 5 minutes, followed by suction filtration and drying at 70°C for 30 minutes. The silver-based activator is a silver ammonia solution with a concentration of 10 g / L; The mass ratio of the silver-based activator to pure water is 1:(1-5); The volume ratio of the carbon fiber powder described in step 1 to the silver-based activator described in step 3 is 1g:(20mL-25mL); Fourth, CuSO4.5H2O, potassium sodium tartrate and EDTA-2Na are added to pure water and mixed and stirred, and then NaOH is added to adjust the solution to a pH of 11.5-12.5, and then placed in a water bath at 70°C-75°C, and formaldehyde solution is added dropwise, and then the product dried in step 3 is added, and heated in a water bath at 70°C-75°C for 5min-6min, the solution changes from dark blue to white, and finally filtered and dried in sequence to obtain copper-plated carbon fiber powder, and the thickness of the copper plating layer is 6μm-9μm; The mass fraction of the formaldehyde solution is 37%; The volume ratio of the formaldehyde solution to pure water is 1:(25-50); The mass ratio of potassium sodium tartrate to CuSO4.5H2O is 1:(1.3-1.5); The mass ratio of potassium sodium tartrate to EDTA-2Na is 1:(1-1.5); The mass ratio of the potassium sodium tartrate to the volume of pure water is 1g:(25mL-30mL); The mass ratio of the carbon fiber powder described in step one to the potassium sodium tartrate described in step four is 1:(6-12).

4. A method for partial transient liquid phase bonding of silicon nitride ceramics / nickel-based high-temperature alloys according to claim 1, characterized in that The rotation speed of the low-speed ball mill in step 1 is 100 r / min.

5. A method for partial transient liquid phase bonding of silicon nitride ceramics / nickel-based high-temperature alloys according to claim 1, characterized in that The pressure of the tablet press in step 1 is 2MPa.

6. A method for partial transient liquid phase bonding of silicon nitride ceramics / nickel-based high-temperature alloys according to claim 1, characterized in that The method for pre-treating the base material nickel-based alloy in step 2 is as follows: the base material nickel-based alloy is treated with water sandpaper to remove the oxide layer and coarse scratches visible to the naked eye on the metal surface, and then polished with 600#, 800#, and 1000# metallographic sandpapers in sequence until there are no obvious scratches on the surface, and finally polished with diamond particles with a particle size of 0.5μm to make the surface to be welded bright; finally, it is ultrasonically cleaned with anhydrous ethanol for 10 minutes and dried for later use.

7. A method for partial transient liquid phase bonding of silicon nitride ceramics / nickel-based high temperature alloys according to claim 1, characterized in that The parent nickel-based alloy is GH4169 nickel-based alloy.

8. A method for partial transient liquid phase bonding of silicon nitride ceramics / nickel-based high temperature alloys according to claim 1, characterized in that The method for pre-treating the base material silicon nitride ceramic block in step 2 is as follows: coarsely grind the silicon nitride ceramic block on a 400# diamond grinding disc until the surface of the sample is flat, then use W3.5 diamond grinding paste to grind on a flat glass until there are no obvious wire cutting marks on the silicon nitride welding surface, then use W1 grinding paste to grind until the surface of the silicon nitride ceramic is bright, and finally use anhydrous ethanol ultrasonic cleaning for 10 minutes, and dry for use.

9. A method for partial transient liquid phase bonding of silicon nitride ceramics / nickel-based high temperature alloys according to claim 1, characterized in that The adhesive described in step three is 502 glue.

10. A method for partial transient liquid phase bonding of silicon nitride ceramics / nickel-based high temperature alloys according to claim 1, characterized in that In step 4, the sandwich structure to be welded assembled in step 3 is placed in a vacuum heating furnace, and the temperature is first increased from room temperature to 300°C~310°C at a heating rate of 10°C / min and kept warm for 30 minutes to ensure that the adhesive is completely volatilized, and then the temperature is increased to 1000°C~1060°C at a heating rate of 10°C / min and kept warm for 5 minutes to 20 minutes; then the temperature is reduced to 300°C~310°C at a cooling rate of 5°C / min, and finally naturally cooled to room temperature to complete the brazing process; the entire process of step 4 is carried out under vacuum conditions.

Citation Information

Patent Citations

  • Carbon fiber-reinforced aluminum-magnesium alloy composite material and preparation method thereof

    CN104213056A

  • Welding method for relieving residual stress of ceramic and metal brazed joint

    CN110883397A

  • Indirect brazing method for aluminum nitride ceramic copper-clad plate

    CN113307647A

  • Solder foil, semiconductor device and electronic device

    JP2002301588A