Flexible bendable tungsten electrode and preparation method thereof

The flexible bendable tungsten electrode prepared through specific ratios and process flow solves the problem of breakage in use and transportation of tungsten electrodes, and maintains excellent welding performance, which is suitable for a variety of industrial fields.

CN118951489APending Publication Date: 2024-11-15SHANDONG MAIKE TUNGSTEN MOLYBDENUM TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411139742.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing tungsten electrodes are prone to break due to pressure or bending during use and transportation, and the welding performance is difficult to take into account both flexibility and strength, which cannot meet the modern industry's demand for flexible bendable electrodes.

Method used

Using specific ratios of potassium oxide, silicon oxide, aluminum nitrate, rare earth oxide and tungsten powder, flexible with high plasticity is prepared through hydrogen reduction, drying, mixing, blanking, sintering, rotary forging and drawing processes. The bendable tungsten electrode can be bent at 0-180° and maintain excellent welding performance.

Benefits of technology

It realizes high shaping and toughness of tungsten electrodes, avoids fracture, and maintains excellent welding performance, simplifies process flow, improves production efficiency and energy efficiency, and is suitable for a variety of industrial fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118951489A_ABST
    Figure CN118951489A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of tungsten electrode preparation, in particular to a flexible bendable tungsten electrode and a preparation method thereof.The tungsten electrode comprises, by weight, 0.1 wt%-0.3 wt% of potassium oxide, 0.05 wt%-0.25 wt% of silicon dioxide, 0.03 wt%-0.2 wt% of aluminum nitrate, 0.1 wt%-3.2 wt% of rare earth oxide and the balance tungsten powder; the tungsten electrode has high plasticity and can be flexibly bent by 0-180 degrees; the tungsten electrode prepared by the process has the same excellent welding performance; the preparation method is simple, the technological process is coherent, and the production efficiency can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tungsten electrode preparation, and in particular to a flexible and bendable tungsten electrode and a preparation method thereof. Background Art

[0002] Gas tungsten arc welding, or tungsten inert gas welding, is an arc welding method that uses a non-melting tungsten electrode for welding. It is commonly used to weld thin plates of stainless steel and non-ferrous metals such as aluminum, magnesium, and copper alloys. It is mainly used in the aerospace industry, but many industries also use it to weld thin workpieces, especially non-ferrous metals.

[0003] However, the current research direction of tungsten electrodes is too single, mainly focusing on the welding performance of the electrodes, while ignoring their own comprehensive performance. Generally speaking, materials with high strength also have high hardness, but this usually leads to reduced plasticity. As we all know, tungsten is one of the hardest metals, second only to chromium, which also means that tungsten has extremely low plasticity among metals, which means that tungsten is more prone to brittle fracture when subjected to force. Therefore, the use and transportation of tungsten electrodes on the market must prevent the tungsten electrodes from bending and being compressed. At the same time, with the development of the industry, many special and precise operating scenarios and ecological scenarios have also been added, which require welding through flexible electrodes.

[0004] In addition, the tungsten electrode itself is a welding consumable, so changes in the composition and technical improvements of the tungsten electrode cannot reduce its welding performance. In summary, finding a flexible and bendable tungsten electrode that has sufficient plasticity, can be flexibly bendable, and does not affect its welding performance has become the current industry market demand. Summary of the invention

[0005] The purpose of the present invention is to provide a flexible bendable tungsten electrode to solve the problems existing in the prior art. The tungsten electrode has high plasticity, can be bent by 0-180 degrees, and has excellent welding performance.

[0006] The present invention adopts the following technical solution: A flexible and bendable tungsten electrode, the tungsten electrode composition includes potassium oxide, silicon dioxide, aluminum nitrate, rare earth oxide and tungsten powder, the specific weight ratio is: Potassium oxide content: 0.1wt%-0.3wt%, Silicon dioxide content: 0.05wt%-0.25wt%, Aluminum nitrate content: 0.03wt%-0.2wt%, Rare earth oxide content: 0.1wt%-3.2wt%, The remainder is tungsten powder.

[0007] Furthermore, the tungsten electrode composition includes potassium oxide, silicon dioxide, aluminum nitrate, rare earth oxide and tungsten powder, and the weight ratio is specifically as follows: Potassium oxide content is 0.12wt%, The silicon dioxide content is 0.08wt%, Aluminum nitrate content is 0.08wt%, Rare earth oxides are 2.2wt%, The balance is tungsten powder.

[0008] Furthermore, the rare earth oxide is one or more of lanthanum oxide, cerium oxide, and yttrium oxide.

[0009] Another object of the present invention is to provide a method for preparing a flexible and bendable tungsten electrode, comprising the following steps: (1) Preparing potassium silicate and aluminum nitrate solutions: convert the weight of potassium oxide into the weight of potassium hydroxide, weigh potassium hydroxide, and mix potassium hydroxide and water in a weight ratio of 1:50 to obtain a potassium hydroxide solution; convert the weight of silicon dioxide into the weight of silicic acid, weigh silicic acid and add it to the potassium hydroxide solution to obtain a potassium silicate solution; weigh aluminum nitrate, and mix aluminum nitrate and water in a weight ratio of 1:30 to obtain an aluminum nitrate solution for later use; (2) adding the potassium silicate and aluminum nitrate solution obtained in step (1) to the blue tungsten powder for solid-liquid doping, and mixing thoroughly to obtain a mixed solution; (3) Reduction: The mixed liquid is placed in a hydrogen reduction furnace to reduce the oxide in the blue tungsten powder to tungsten powder to obtain reduced tungsten powder; (4) Drying: The reduced tungsten powder is placed in a drying furnace to dry the residual solvent and moisture in the tungsten powder to obtain dried tungsten powder; (5) Mixing: The dried tungsten powder and rare earth oxide are mixed by solid-solid doping in a mixer; (6) Pressing: The mixed tungsten powder is loaded into a mold and pressure is applied to the tungsten powder by a press to obtain a preform; (7) Sintering: Place the preform into a medium frequency sintering furnace for sintering to obtain a sintered tungsten bar; (8) Rotary forging: The tungsten bar is rotary forged by a rotary forging machine to reduce its diameter. The rotary forging speed is 12 m / min. (9) Chain drawing: The tungsten rod is drawn twice by a double-chain drawing machine and once by a single-chain drawing machine to form a tungsten wire with a diameter of 1.0 mm to 3.0 mm; (10) Straightening and cutting: The tungsten wire after chain pulling is straightened by a straightening machine, and then cut to a fixed length according to the length of the tungsten electrode; (11) Cleaning and packaging: The straightened and double-cut tungsten electrode is cleaned and packaged to obtain the final flexible and bendable tungsten electrode.

[0010] Furthermore, in step (3), the hydrogen flow rate is adjusted to 400 m³ / h, the reduction temperature is adjusted to 1050°C, and maintained for 12h-15h.

[0011] Furthermore, in step (3), the drying temperature is adjusted to 100° C.-200° C., and the drying time is adjusted to 10 h-43 h.

[0012] Furthermore, the mixing time in step (5) is 4-5 h.

[0013] Furthermore, the pressure in step (6) is set to 170 MPa.

[0014] Furthermore, the sintering temperature in step (7) is 1500° C.-2000° C., and the sintering time is 20 h-28 h.

[0015] Furthermore, in step (9), the drawing temperature is 800° C. and the drawing speed is 30 m / min.

[0016] The beneficial effects of the present invention are as follows: (1) The tungsten electrode of the present invention has high plasticity and can be flexibly bent: on the basis of the original chemical composition of the tungsten electrode, specific elements are added, and the tungsten electrode prepared by a specific process has higher plasticity and toughness, which can effectively avoid the phenomenon that the tungsten electrode is broken and cannot be used due to pressure or bending during use and transportation; (2) The tungsten electrode of the present invention has excellent welding performance: the welding performance of the tungsten electrode mainly comes from the addition of rare earth oxides to metal tungsten to stimulate its electronic work function, so that the welding performance of the tungsten electrode is improved. The tungsten electrode prepared by the process of the present invention has equally excellent welding performance; (3) The preparation method of the present invention is simple and has a coherent process flow, which can significantly improve production efficiency and reduce energy consumption in the preparation process, meeting the requirements of high efficiency and energy saving in modern industrial production; (4) The tungsten electrode of the present invention has broad application prospects: Due to its excellent plasticity, flexibility and bendability, the tungsten electrode of the present invention can also be applied to the fields of electronics, chemical industry, metallurgy, heat treatment, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The metallographic structure diagram of the longitudinal section of the commercially available tungsten electrode with the specification of Φ3.0mm*175mm×200; Figure 2 The metallographic structure diagram of the longitudinal section of the tungsten electrode with a specification of Φ3.0mm*175mm×200 obtained in Example 3 of the present invention. DETAILED DESCRIPTION

[0018] In order to enable those skilled in the art to better understand the present invention, the technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0019] Embodiment 1 A flexible and bendable tungsten electrode comprises potassium oxide, silicon dioxide, aluminum nitrate, rare earth oxide and tungsten powder, wherein the weight ratio is as follows: Potassium oxide content: 0.1wt%, Silicon dioxide content: 0.25wt%, Aluminum nitrate content: 0.2wt%, Rare earth oxide (yttrium oxide) content: 0.1wt%, The remainder is tungsten powder.

[0020] The preparation method of the tungsten electrode comprises the following steps: (1) Preparing potassium silicate and aluminum nitrate solutions: convert the weight of potassium oxide into the weight of potassium hydroxide, weigh potassium hydroxide, and mix potassium hydroxide and water in a weight ratio of 1:50 to obtain a potassium hydroxide solution; convert the weight of silicon dioxide into the weight of silicic acid, weigh silicic acid and add it to the potassium hydroxide solution to obtain a potassium silicate solution; weigh aluminum nitrate, and mix aluminum nitrate and water in a weight ratio of 1:30 to obtain an aluminum nitrate solution for later use; (2) adding the potassium silicate and aluminum nitrate solution obtained in step (1) to the blue tungsten powder for solid-liquid doping, and mixing thoroughly to obtain a mixed solution; (3) Reduction process: Use hydrogen reduction to make alloy powder. Put the doped blue tungsten powder into the hydrogen reduction furnace, adjust the hydrogen flow rate to 400m³ / h, adjust the reduction temperature to 1050℃, and maintain it for 12h to reduce the oxide in the blue tungsten powder to tungsten powder, and obtain the reduced tungsten powder; (4) Drying process: Place the reduced tungsten powder into a drying furnace, adjust the drying temperature to 100°C, and dry the residual solvent and water in the tungsten powder for 10 hours to obtain dried tungsten powder; (5) Mixing process: The alloy powder and rare earth oxide are solid-solid doped by a mixer, and the mixing time is 4 hours; (6) Pressing process: The dried tungsten powder is loaded into a mold and pressure is applied to the tungsten powder by a press machine. The pressure is set to 170 MPa to form a preform of a certain shape and size. (7) Sintering process: Place the preform into a medium frequency sintering furnace, adjust the temperature to 1700°C, and sinter for 20 hours to obtain a sintered tungsten bar; (8) Rotary forging process: The tungsten bar is rotary forged by a rotary forging machine to reduce its diameter, and the rotary forging speed is 12 m / min; (9) Chain drawing: double chain one-time drawing, double chain two-time drawing, single chain drawing. The tungsten rod is drawn twice by a double chain drawing machine and once by a single chain drawing machine, so that the tungsten rod forms a tungsten electrode with a diameter of 1.0mm-3.0mm. The drawing temperature is 800℃ and the speed is 30m / min. (10) Straightening and cutting: The tungsten wire after chain pulling is straightened by a straightening machine, and then cut to a fixed length according to the length of the tungsten electrode; (11) Cleaning and packaging: The straightened and double-cut tungsten electrode is cleaned to remove grease and impurities on the surface, and then packaged to obtain the final flexible and bendable tungsten electrode.

[0021] Embodiment 2 A flexible and bendable tungsten electrode comprises potassium oxide, silicon dioxide, aluminum nitrate, rare earth oxide and tungsten powder, wherein the weight ratio is as follows: Potassium oxide content: 0.3wt%, Silicon dioxide content: 0.05wt%, Aluminum nitrate content: 0.03wt%, Rare earth oxide (cerium oxide and lanthanum oxide, weight ratio 1:1.2) content: 3.2wt%, The remainder is tungsten powder.

[0022] The preparation method of the tungsten electrode comprises the following steps: (1) Preparing potassium silicate and aluminum nitrate solutions: convert the weight of potassium oxide into the weight of potassium hydroxide, weigh potassium hydroxide, and mix potassium hydroxide and water in a weight ratio of 1:50 to obtain a potassium hydroxide solution; convert the weight of silicon dioxide into the weight of silicic acid, weigh silicic acid and add it to the potassium hydroxide solution to obtain a potassium silicate solution; weigh aluminum nitrate, and mix aluminum nitrate and water in a weight ratio of 1:30 to obtain an aluminum nitrate solution for later use; (2) adding the potassium silicate and aluminum nitrate solution obtained in step (1) to the blue tungsten powder for solid-liquid doping, and mixing thoroughly to obtain a mixed solution; (3) Reduction process: Use hydrogen reduction to make alloy powder. Put the doped blue tungsten powder into the hydrogen reduction furnace, adjust the hydrogen flow rate to 400m³ / h, adjust the reduction temperature to 1050℃, and maintain it for 15h to reduce the oxide in the blue tungsten powder to tungsten powder, and obtain the reduced tungsten powder; (4) Drying process: Place the reduced tungsten powder into a drying furnace, adjust the drying temperature to 170°C, and dry the residual solvent and water in the tungsten powder for 43 hours to obtain dried tungsten powder; (5) Mixing process: The alloy powder and rare earth oxide are solid-solid doped by a mixer, and the mixing time is 4.5 h; (6) Pressing process: The dried tungsten powder is loaded into a mold and pressure is applied to the tungsten powder by a press machine. The pressure is set to 170 MPa to form a preform of a certain shape and size. (7) Sintering process: Place the preform into a medium frequency sintering furnace, adjust the temperature to 1500°C, and sinter for 28 hours to obtain a sintered tungsten bar; (8) Rotary forging process: The tungsten bar is rotary forged by a rotary forging machine to reduce its diameter, and the rotary forging speed is 12 m / min; (9) Chain drawing: double chain one-time drawing, double chain two-time drawing, single chain drawing. The tungsten rod is drawn twice by a double chain drawing machine and once by a single chain drawing machine, so that the tungsten rod forms a tungsten electrode with a diameter of 1.0mm-3.0mm. The drawing temperature is 800℃ and the speed is 30m / min. (10) Straightening and cutting: The tungsten wire after chain pulling is straightened by a straightening machine, and then cut to a fixed length according to the length of the tungsten electrode; (11) Cleaning and packaging: The straightened and double-cut tungsten electrode is cleaned to remove grease and impurities on the surface, and then packaged to obtain the final flexible and bendable tungsten electrode.

[0023] Embodiment 3 A flexible and bendable tungsten electrode, the tungsten electrode composition includes potassium oxide, silicon dioxide, aluminum nitrate, rare earth oxide and tungsten powder, specifically in the following weight ratio: Potassium oxide content is 0.12wt%, The silicon dioxide content is 0.08wt%, Aluminum nitrate content is 0.08wt%, Rare earth oxide (cerium oxide) is 2.2wt%, The balance is tungsten powder.

[0024] The preparation method of the tungsten electrode comprises the following steps: (1) Preparing potassium silicate and aluminum nitrate solutions: convert the weight of potassium oxide into the weight of potassium hydroxide, weigh potassium hydroxide, and mix potassium hydroxide and water in a weight ratio of 1:50 to obtain a potassium hydroxide solution; convert the weight of silicon dioxide into the weight of silicic acid, weigh silicic acid and add it to the potassium hydroxide solution to obtain a potassium silicate solution; weigh aluminum nitrate, and mix aluminum nitrate and water in a weight ratio of 1:30 to obtain an aluminum nitrate solution for later use; (2) adding the potassium silicate and aluminum nitrate solution obtained in step (1) to the blue tungsten powder for solid-liquid doping, and mixing thoroughly to obtain a mixed solution; (3) Reduction process: Use hydrogen reduction to make alloy powder. Put the doped blue tungsten powder into the hydrogen reduction furnace, adjust the hydrogen flow rate to 400m³ / h, adjust the reduction temperature to 1050℃, and maintain it for 13h to reduce the oxide in the blue tungsten powder to tungsten powder, and obtain the reduced tungsten powder; (4) Drying process: Place the reduced tungsten powder into a drying furnace, adjust the drying temperature to 200°C, and dry the residual solvent and water in the tungsten powder for 24 hours to obtain dried tungsten powder; (5) Mixing process: The alloy powder and rare earth oxide are solid-solid doped by a mixer, and the mixing time is 5 hours; (6) Pressing process: The dried tungsten powder is loaded into a mold and pressure is applied to the tungsten powder by a press machine. The pressure is set to 170 MPa to form a preform of a certain shape and size. (7) Sintering process: Place the preform into a medium frequency sintering furnace, adjust the temperature to 2000°C, and sinter for 23 hours to obtain a sintered tungsten bar; (8) Rotary forging process: The tungsten bar is rotary forged by a rotary forging machine to reduce its diameter, and the rotary forging speed is 12 m / min; (9) Chain drawing: double chain one-time drawing, double chain two-time drawing, single chain drawing. The tungsten rod is drawn twice by a double chain drawing machine and once by a single chain drawing machine, so that the tungsten rod forms a tungsten electrode with a diameter of 1.0mm-3.0mm. The drawing temperature is 800℃ and the speed is 30m / min. (10) Straightening and cutting: The tungsten wire after chain pulling is straightened by a straightening machine, and then cut to a fixed length according to the length of the tungsten electrode; (11) Cleaning and packaging: The straightened and double-cut tungsten electrode is cleaned to remove grease and impurities on the surface, and then packaged to obtain the final flexible and bendable tungsten electrode.

[0025] Comparative Example 1 Compared with Example 3, the difference of Comparative Example 1 is that in the reduction process of step (3) of the preparation method, the hydrogen flow rate is adjusted to 300 m³ / h, and the reduction temperature is adjusted to 900° C.; other parameters and operations are the same as those of Example 3.

[0026] Comparative Example 2 Compared with Example 3, the difference of Comparative Example 2 is that in the green compacting process of step (6) of the preparation method, the pressure is set to 150 MPa; the other parameters and operations are the same as those of Example 3.

[0027] Comparative Example 3 Compared with Example 3, the difference of Comparative Example 3 is that in the sintering process of step (7) of the preparation method, the temperature is 1400° C. and the sintering time is 18 h; other parameters and operations are the same as those of Example 3.

[0028] Comparative Example 4 A flexible and bendable tungsten electrode, the tungsten electrode composition includes silicon dioxide, aluminum nitrate, rare earth oxide and tungsten powder, the specific weight ratio is: The silicon dioxide content is 0.08wt%, Aluminum nitrate content is 0.08wt%, Rare earth oxide (cerium oxide) is 2.2wt%, The balance is tungsten powder.

[0029] The preparation method of the tungsten electrode comprises the following steps: (1) preparing an aluminum nitrate solution: weighing aluminum nitrate, and mixing aluminum nitrate with water in a weight ratio of 1:30 to prepare an aluminum nitrate solution for later use; (2) solid-liquid doping the silicon dioxide, the aluminum nitrate solution obtained in step (1) and the blue tungsten powder, and fully mixing them to obtain a mixed solution; Other parameters and operations are the same as those in Example 3.

[0030] Comparative Example 5 A flexible and bendable tungsten electrode, the tungsten electrode composition includes ammonium rhenate, molybdenum powder, rare earth oxide and tungsten powder, and the specific weight ratio is: The content of ammonium rhenate is 0.3wt%, The molybdenum powder content is 0.08wt%, The rare earth oxides (cerium oxide and yttrium oxide, the weight ratio of the two is 2:1) are 3.3wt%, The balance is tungsten powder.

[0031] The preparation method of the tungsten electrode comprises the following steps: (1) preparing an ammonium rhenate solution: weighing ammonium rhenate, and mixing ammonium rhenate with water in a weight ratio of 1:30 to prepare an ammonium rhenate solution for later use; (2) solid-liquid doping the ammonium rhenate solution obtained in step (1) with molybdenum powder and blue tungsten powder, and fully mixing them to obtain a mixed solution; Other parameters and operations are the same as those in Example 3.

[0032] Comparative Example 6 A flexible and bendable tungsten electrode, the tungsten electrode composition includes aluminum nitrate, rare earth oxide and tungsten powder, the specific weight ratio is: Aluminum nitrate content is 0.08wt%, Rare earth oxide (cerium oxide) is 2.2wt%, The balance is tungsten powder.

[0033] (1) preparing an aluminum nitrate solution: weighing aluminum nitrate, and mixing aluminum nitrate with water in a weight ratio of 1:30 to prepare an aluminum nitrate solution for later use; (2) adding the aluminum nitrate solution obtained in step (1) to the blue tungsten powder for solid-liquid doping, and mixing thoroughly to obtain a mixed solution; Other parameters and operations are the same as those in Example 3.

[0034] Test Examples The welding performance and bending performance of the tungsten electrodes obtained in Examples 1-3 and Comparative Examples 1-6 were tested.

[0035] Among them, (1) welding performance testing method is as follows: The welding performance of the samples was verified by an oxygen arc welding machine. The welding performance mainly includes arc starting performance, arc starting stability, and anti-burning performance. Among the welding performance, arc starting performance and arc starting stability belong to qualitative evaluation. Since the welding level of the welding experimenter affects the evaluation results to a certain extent, the samples were evaluated for arc starting performance and arc starting stability by the same welder with rich welding experience. The anti-burning performance is a quantitative evaluation. The weight loss of the sample after 20 minutes of welding was examined under the conditions of welding current 160A and argon gas flow rate 10L / min.

[0036] (2) The bending degree detection method is as follows: The bending performance of the sample was verified by a universal testing machine. The method was based on YB / T 5349-2006 (Metal Bending Mechanical Performance Test Method). The three-point bending test was selected. The specimen was placed on two supporting points at a certain distance. A downward load was applied to the specimen at the midpoint of the two supporting points. When the three contact points of the specimen formed two equal moments, three-point bending occurred, and the specimen would break at the midpoint. The bending angle was then calculated based on the deflection and tungsten electrode length data.

[0037] Table 1 Comparison of product performance of Examples 1-3 and Comparative Examples 1-6 .

[0038] It can be seen from the data in Table 1 that the tungsten electrode obtained in the embodiment of the present invention is significantly better than the comparative example in terms of welding performance and bending degree. Among them, embodiment 3 is the best embodiment.

[0039] The tungsten electrode obtained in Example 3 was made into a size of Φ3.0mm*175mm, and its longitudinal section ×200 metallographic structure diagram ( Figure 2 As shown in the figure), the longitudinal section × 200 metallographic structure diagram of the same specification WC20 tungsten electrode (manufacturer: Guangdong Zhonghuan New Material Technology Co., Ltd.) on the market is also compared with the longitudinal section × 200 metallographic structure diagram of the same specification WC20 tungsten electrode (manufacturer: Guangdong Zhonghuan New Material Technology Co., Ltd.) Figure 1 as shown) for comparison.

[0040] From the comparison of the pictures, we can see that the longitudinal section of the cerium tungsten electrode with the same finished product specification of Φ3.0mm*175mm×200 metallographic structure is shown in the figure above. By comparison, it can be found that the cerium tungsten electrode with silicon, aluminum and potassium elements added has many black spots on the grain boundaries of the texture organization. This is because the silicon, aluminum and potassium elements evaporate during the production process of the tungsten electrode and leave potassium bubbles. These potassium bubbles are densely distributed on the grain boundaries of the texture organization, thereby preventing the grains from growing longitudinally, so that the texture organization can only grow horizontally, and finally form a more developed texture organization.

[0041] By comparing the metallographic pictures, it can be easily concluded that the texture of WC20 with the addition of silicon, aluminum and potassium elements is significantly more developed than that of normal WC20, and the more developed fiber structure can effectively improve the shaping of the tungsten electrode, thereby greatly reducing the possibility of brittle fracture of the tungsten electrode when it is bent.

[0042] From the comparison of the data and pictures in Table 1, it can be seen that the tungsten electrode prepared by the specific raw materials, proportions and specific process flow in the present invention has higher plasticity and toughness, and can effectively avoid the phenomenon that the tungsten electrode is broken and cannot be used due to pressure or bending during use and transportation; the tungsten electrode prepared by the process of the present invention has equally good welding performance; the preparation method of the present invention is simple and the process flow is coherent, which can significantly improve production efficiency and reduce energy consumption in the preparation process, meeting the requirements of high efficiency and energy saving in modern industrial production.

Claims

1. A flexible and bendable tungsten electrode, characterized in that: The tungsten electrode comprises potassium oxide, silicon dioxide, aluminum nitrate, rare earth oxide and tungsten powder, and the specific weight ratio is: Potassium oxide content: 0.1wt%-0.3wt%, Silicon dioxide content: 0.05wt%-0.25wt%, Aluminum nitrate content: 0.03wt%-0.2wt%, Rare earth oxide content: 0.1wt%-3.2wt%, The remainder is tungsten powder.

2. A flexible bendable tungsten electrode according to claim 1, characterized in that: The tungsten electrode comprises potassium oxide, silicon dioxide, aluminum nitrate, rare earth oxide and tungsten powder, and the specific weight ratio is: Potassium oxide content is 0.12wt%, The silicon dioxide content is 0.08wt%, Aluminum nitrate content is 0.08wt%, Rare earth oxides are 2.2wt%, The balance is tungsten powder.

3. A flexible bendable tungsten electrode according to any one of claims 1-2, characterized in that: The rare earth oxide is one or more of lanthanum oxide, cerium oxide and yttrium oxide.

4. A method for preparing a flexible bendable tungsten electrode as claimed in claims 1 to 3, characterized in that: The steps include: (1) Preparing potassium silicate and aluminum nitrate solutions: convert the weight of potassium oxide into the weight of potassium hydroxide, weigh potassium hydroxide, and mix potassium hydroxide and water in a weight ratio of 1:50 to obtain a potassium hydroxide solution; convert the weight of silicon dioxide into the weight of silicic acid, weigh silicic acid and add it to the potassium hydroxide solution to obtain a potassium silicate solution; weigh aluminum nitrate, and mix aluminum nitrate and water in a weight ratio of 1:30 to obtain an aluminum nitrate solution for later use; (2) adding the potassium silicate and aluminum nitrate solution obtained in step (1) to the blue tungsten powder for solid-liquid doping, and mixing thoroughly to obtain a mixed solution; (3) Reduction: The mixed liquid is placed in a hydrogen reduction furnace to reduce the oxide in the blue tungsten powder to tungsten powder, thereby obtaining reduced tungsten powder; (4) Drying: The reduced tungsten powder is placed in a drying furnace to dry the residual solvent and moisture in the tungsten powder to obtain dried tungsten powder; (5) Mixing: The dried tungsten powder and rare earth oxide are mixed by solid-solid doping in a mixer; (6) Pressing: The mixed tungsten powder is loaded into a mold and pressure is applied to the tungsten powder by a press to obtain a preform; (7) Sintering: Place the preform into a medium frequency sintering furnace for sintering to obtain a sintered tungsten bar; (8) Rotary forging: The tungsten bar is rotary forged by a rotary forging machine to reduce its diameter. The rotary forging speed is 12 m / min. (9) Chain drawing: The tungsten rod is drawn twice by a double-chain drawing machine and once by a single-chain drawing machine to form a tungsten wire with a diameter of 1.0 mm to 3.0 mm; (10) Straightening and cutting: The tungsten wire after chain pulling is straightened by a straightening machine, and then cut to a fixed length according to the length of the tungsten electrode; (11) Cleaning and packaging: The straightened and double-cut tungsten electrode is cleaned and packaged to obtain the final flexible and bendable tungsten electrode.

5. The method for preparing a flexible bendable tungsten electrode according to claim 4, characterized in that: In step (3), the hydrogen flow rate is adjusted to 400 m³ / h, and the reduction temperature is adjusted to 1050°C and maintained for 12h-15h.

6. The method for preparing a flexible bendable tungsten electrode according to claim 4, characterized in that: In step (3), the drying temperature is adjusted to 100° C.-200° C., and the drying time is adjusted to 10 h-43 h.

7. The method for preparing a flexible bendable tungsten electrode according to claim 4, characterized in that: The mixing time in step (5) is 4-5 h.

8. The method for preparing a flexible bendable tungsten electrode according to claim 4, characterized in that: The pressure in step (6) is set to 170 MPa.

9. The method for preparing a flexible bendable tungsten electrode according to claim 4, characterized in that: The sintering temperature in step (7) is 1500° C.-2000° C., and the sintering time is 20 h-28 h.

10. The method for preparing a flexible bendable tungsten electrode according to claim 4, characterized in that: The drawing temperature in step (9) is 800° C. and the drawing speed is 30 m / min.

Citation Information

Cited By

  • Composite dispersion strengthened tungsten alloy and preparation method thereof

    CN119640077A

  • A composite dispersion strengthened tungsten alloy and its preparation method

    CN119640077B