Three-layer co-extrusion PSU film and preparation method thereof
By introducing modified glass powder and antioxidants into the PSU film, combined with the three-layer coextrusion process, the aging problem of PSU film in a strong ultraviolet environment is solved, and its UV resistance and mechanical properties are improved. It is suitable for high temperature and strong ultraviolet rays Application of the environment.
Patent Information
- Application Number
- CN202411006226.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-25
AI Technical Summary
PSU films are prone to aging in strong ultraviolet environments, resulting in poor application effects, especially when film materials are made, their UV resistance is insufficient.
A three-layer coextruded PSU film structure is adopted, which includes a PSU layer and two modified PSU layers. The modified PSU layer is composed of PSU resin, modified glass powder and antioxidant. The modified glass powder is adhered to the glass powder through PESU resin. The surface is improved, and is prepared by a three-layer coextrusion process to maintain mechanical properties.
It significantly improves the UV resistance and mechanical properties of the PSU film, reduces the agglomeration and unevenness of the glass powder, affects the light transmittance, and is suitable for high-temperature and strong ultraviolet environments.
Smart Images

Figure CN118952791A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of polymer film materials, and in particular to a three-layer co-extruded PSU film and a preparation method thereof. Background Art
[0002] Polysulfone is a kind of aromatic non-crystalline high-performance thermoplastic engineering plastics containing sulfone groups on the main chain of the molecule. Common polysulfones include PESU, PSU and PPSU. Among them, PESU refers to polyethersulfone, PSU refers to bisphenol A polysulfone, and PPSU refers to polyphenylsulfone.
[0003] Bisphenol A type polysulfone PSU is made of bisphenol A and 4,4'-dichlorodiphenyl sulfone as raw materials through polycondensation reaction. Bisphenol A type polysulfone PSU has good mechanical properties, especially under high temperature conditions, the mechanical properties retention rate is high, so it can be used in electronics and electrical applications in the direction of small size, light weight and high temperature resistance.
[0004] However, in more severe environments, such as those with strong ultraviolet rays, PSU is prone to aging, especially for PSU membranes made into film materials, the application effect is not good. Summary of the invention
[0005] In order to improve the UV aging resistance of the PSU film, the present application provides a three-layer co-extruded PSU film and a preparation method thereof.
[0006] In the first aspect, the present application provides a three-layer co-extruded PSU film using the following technical solution: A three-layer co-extruded PSU film comprises a PSU layer and two modified PSU layers, wherein the PSU layer is arranged between the two modified PSU layers, and the modified PSU layer is prepared from raw materials comprising the following parts by weight: PSU resin 100 parts; 3-4.5 parts of modified glass powder; 0.7-1.2 parts of antioxidant; The modified glass powder is obtained by attaching PESU resin to the surface of the glass powder.
[0007] By adopting the above technical scheme, the glass powder has a good ability to absorb and scatter ultraviolet rays. By adding glass powder to the modified PSU layer, the modified PSU layer can block ultraviolet rays, which can improve the ultraviolet resistance of the PSU film. In addition, glass powder is only added to the two layers on the surface of the PSU film. The middle PSU layer effectively maintains the mechanical properties of the PSU film, making the comprehensive performance of the PSU film more excellent.
[0008] The modified glass powder obtained by precipitating and attaching PESU resin to the surface of the glass powder has increased interfacial bonding strength with the PSU resin, reduced glass powder agglomeration, improved the dispersion uniformity of the glass powder, further improved the UV resistance and mechanical properties of the PSU film, and the dispersed modified glass powder has little effect on the light transmittance of the PSU film.
[0009] Optionally, the raw materials for preparing the modified glass powder include glass powder, PESU resin, ether, water and dimethylacetamide, and the mass ratio of the glass powder, PESU resin, ether, water and dimethylacetamide is 1:(0.1-0.25):(3-5):(6-10):(2-4).
[0010] By adopting the above technical scheme, the PESU resin has a similar structure to the PSU resin, so that the compatibility between the surface of the modified glass powder and the PSU resin matrix is improved, thereby improving the interfacial bonding force between the two. In addition, the PESU resin has good flexibility, which promotes the embedding of the surface of the modified glass powder with the PSU resin and maintains the good mechanical properties of the PSU film.
[0011] Optionally, the modified glass powder is prepared by dissolving PESU resin in dimethylacetamide, adding glass powder to dimethylacetamide, first adding ether dropwise, stirring evenly, then adding water dropwise, stirring evenly, separating, and obtaining the modified glass powder.
[0012] By adopting the above technical scheme, utilizing the polarity difference among ether, water and dimethylacetamide and the solubility difference to PESU, ether causes PESU to gradually precipitate and adhere to the surface of glass powder, and water promotes the stable adhesion of PESU, thereby obtaining modified glass powder.
[0013] Optionally, the glass powder has a particle size of 1 to 5 μm.
[0014] By adopting the above technical solution, the glass powder has better transparency, controls the particle size of the glass powder, promotes full dispersion of the glass powder, and exerts the ability to absorb and scatter ultraviolet rays.
[0015] Optionally, the molecular weight of the PSU resin is 78,000 to 84,000.
[0016] Optionally, the molecular weight of the PESU resin is 45,000 to 51,000.
[0017] By adopting the above technical solution and using PESU resin with suitable molecular weight, PESU can be well attached to the surface of glass powder to form a wrapped PESU film, thereby improving the compatibility of glass powder and PSU resin.
[0018] Optionally, the thickness ratio of the PSU layer to the modified PSU layer is 8:1.
[0019] By adopting the above technical solution, the PSU layer is composed of pure PSU resin, and the thickness of the above layer structure is matched to improve the UV resistance of the PSU film while maintaining good mechanical properties.
[0020] Optionally, the antioxidant is selected from one or both of antioxidant 1024 and antioxidant DLTP.
[0021] In the second aspect, the present application provides a method for preparing a three-layer co-extruded PSU film using the following technical solution: A method for preparing a three-layer co-extruded PSU film comprises the following steps: PSU resin is dried for later use; PSU resin, modified glass powder and antioxidant are mixed, heated, extruded and granulated to obtain modified PSU particles, and the modified PSU particles are heated to obtain a modified PSU melt; The PSU resin is heated to obtain a PSU melt; The modified PSU melt is distributed to the upper flow channel and the lower flow channel of the die distributor, and the PSU melt is distributed to the middle flow channel of the die distributor. Then the modified PSU melt and the PSU melt are compound co-extruded in the co-extrusion die, and after co-extrusion, they are cast into a film, cooled and shaped to obtain a three-layer co-extruded PSU film.
[0022] By adopting the above technical solution, the PSU film is prepared by a three-layer co-extrusion method, and the inherent advantages of the composite PSU resin and the UV resistance of the modified PSU are combined to obtain a PSU film with better comprehensive performance.
[0023] In summary, this application has the following beneficial effects: 1. The present application sets a modified PSU layer containing modified glass powder. The glass powder has good ability to absorb and scatter ultraviolet rays. Adding glass powder to the modified PSU layer can improve the ultraviolet resistance of the PSU film. In addition, the glass powder is added to only the two layers on the surface of the PSU film. The middle PSU layer effectively maintains the mechanical properties of the PSU film, making the comprehensive performance of the PSU film more excellent. The interfacial bonding strength between the modified glass powder and the PSU resin is increased, and the agglomeration of the glass powder is reduced, which improves the dispersion uniformity of the glass powder, further improves the ultraviolet resistance and mechanical properties of the PSU film, and the dispersed modified glass powder has little effect on the light transmittance of the PSU film.
[0024] 2. The structure of PESU resin is similar to that of PSU resin, which improves the compatibility between the surface of the modified glass powder and the PSU resin matrix, thereby improving the interfacial bonding between the two. In addition, PESU resin has good flexibility, which promotes the intercalation of the surface of the modified glass powder and the PSU resin, and maintains the good mechanical properties of the PSU film. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a layer structure diagram of the three-layer co-extruded PSU film of Example 1 of the present application.
[0026] 1. PSU layer; 2. Modified PSU layer. DETAILED DESCRIPTION
[0027] The following is combined with Figure 1 This application is described in further detail.
[0028] Preparation Example 1 The method for preparing the modified glass powder comprises the following steps: Weigh 500 g of glass powder, 50 g of PESU resin, 1500 g of ether, 3000 g of water, and 1000 g of dimethylacetamide; the particle size of the glass powder is 1-5 μm, and the molecular weight of the PESU resin is 45,000.
[0029] Dissolve PESU resin in dimethylacetamide, then add glass powder to dimethylacetamide, stir and disperse, first add ether dropwise, stir evenly, add water dropwise after the ether is added, stir evenly, continue stirring for 30 minutes after the water is added, terminate the reaction, filter, separate and collect the solid part, wash the solid part with ethanol and water, and dry to obtain modified glass powder.
[0030] Preparation Example 2 The method for preparing the modified glass powder comprises the following steps: Weigh 500 g of glass powder, 125 g of PESU resin, 2500 g of ether, 5000 g of water, and 2000 g of dimethylacetamide; the particle size of the glass powder is 1-5 μm, and the molecular weight of the PESU resin is 51000.
[0031] Dissolve PESU resin in dimethylacetamide, then add glass powder to dimethylacetamide, stir and disperse, first add ether dropwise, stir evenly, add water dropwise after the ether is added, stir evenly, continue stirring for 30 minutes after the water is added, terminate the reaction, filter, separate and collect the solid part, wash the solid part with ethanol and water, and dry to obtain modified glass powder.
[0032] Preparation Example 3 This preparation example is different from preparation example 1 in that the molecular weight of the PESU resin is 92,000.
[0033] Comparative Preparation Example 1 The difference between this comparative preparation example and preparation example 1 is that the PESU resin is replaced by an equal amount of PSU resin, and the molecular weight of the PSU resin is 65,000.
[0034] Comparative Preparation Example 2 The difference between this comparative preparation example and preparation example 1 is that the PESU resin is replaced by an equal amount of PPSU resin, and the molecular weight of the PPSU resin is 60,000.
[0035] Example 1 like Figure 1 As shown, the three-layer co-extruded PSU film includes a PSU layer 1 and two modified PSU layers 2 , and the PSU layer 1 is arranged between the two modified PSU layers 2 .
[0036] The preparation method of the three-layer co-extruded PSU film comprises the following steps: Preparation of modified PSU melt: Weigh 10 kg of PSU resin, 300 g of modified glass powder, and 70 g of antioxidant.
[0037] The molecular weight of the PSU resin is 78,000, the modified glass powder is prepared according to Preparation Example 1, and the antioxidant is composed of antioxidant 1024 and antioxidant DLTP in a mass ratio of 2:3.
[0038] The PSU resin was dried at 140°C for 4 h and set aside.
[0039] The PSU resin, modified glass powder and antioxidant are mixed in a high-speed mixer, and then put into a twin-screw extruder for heating, extrusion and granulation. The extruder temperature is: zone 1 temperature 330°C, zone 2-5 temperature 340°C, die head temperature 340°C to obtain modified PSU particles. The modified PSU particles are then put into a single-screw extruder and heated to 340°C to obtain a modified PSU melt.
[0040] Preparation of PSU melt: Another PSU resin was taken and put into another single-screw extruder and heated to 340° C. to obtain a PSU melt.
[0041] Preparation of three-layer co-extruded PSU film: The modified PSU melt is distributed to the upper flow channel and the lower flow channel of the die distributor, and the PSU melt is distributed to the middle flow channel of the die distributor. Then the modified PSU melt and the PSU melt are compound co-extruded in the co-extrusion die. The die temperature is 340°C. After co-extrusion, the film is cast and cooled and shaped. The modified PSU melt forms a modified PSU layer, and the PSU melt forms a PSU layer to obtain a three-layer co-extruded PSU film.
[0042] The thickness of the three-layer co-extruded PSU film is 150 μm, and the thickness ratio of the PSU layer to the single-layer modified PSU layer is 8:1.
[0043] Example 2 The difference between this embodiment and embodiment 1 is that the raw materials for preparing the modified PSU layer are different.
[0044] The raw materials for preparing the modified PSU layer are: 10kg PSU resin, 450g modified glass powder, 120g antioxidant.
[0045] The molecular weight of the PSU resin is 84000, the modified glass powder is prepared according to Preparation Example 2, and the antioxidant is composed of antioxidant 1024 and antioxidant DLTP in a mass ratio of 2:3.
[0046] Example 3 The difference between this embodiment and embodiment 1 is that the raw materials for preparing the modified PSU layer are different.
[0047] Among the raw materials for preparing the modified PSU layer, the modified glass powder is prepared according to Preparation Example 3.
[0048] Comparative Example 1 The PSU film is prepared from PSU resin, comprising the following steps: Take PSU resin, the molecular weight of which is 78000, put the PSU resin into a single screw extruder and heat it to 340°C to obtain a PSU melt, cast the melt into a film, cool and shape it, and obtain a PSU film, the thickness of the PSU film is 150 μm.
[0049] Comparative Example 2 The difference between this comparative example and Example 1 is that the raw materials for preparing the modified PSU layer are different.
[0050] In this comparative example, the modified glass powder was replaced with an equal amount of glass powder.
[0051] Comparative Example 3 The difference between this comparative example and Example 1 is that the raw materials for preparing the modified PSU layer are different.
[0052] The modified glass powder of this comparative example is prepared by Comparative Preparation Example 1.
[0053] Comparative Example 4 The difference between this comparative example and Example 1 is that the raw materials for preparing the modified PSU layer are different.
[0054] The modified glass powder of this comparative example is prepared by Comparative Preparation Example 2.
[0055] Performance Testing Tensile property test: With reference to GB / T 1040.3-2006 “Determination of tensile properties of plastics Part 3: Test conditions for films and sheets”, the tensile strength and elongation at break of the PSU films prepared in the embodiments and comparative examples were tested. The test results are shown in Table 1.
[0056] Ultraviolet aging test: The PSU membranes prepared in each embodiment and comparative example were placed in a UV aging box. The irradiation light source adopted a UVA-340 ultraviolet fluorescent lamp. The aging temperature was 55°C, the humidity was 80%, and the aging time was 120h. After the aging, the tensile properties of the PSU membranes were tested. The tensile properties of the PSU membranes that had not been tested for aging were compared and the aging retention rate was calculated. The results are shown in Table 1.
[0057] Light transmittance test: Referring to GB / T 2410-2008 “Determination of light transmittance and haze of transparent plastics”, the light transmittance of the PSU films prepared in the embodiments and comparative examples was tested. The test results are shown in Table 1.
[0058] Table 1 From the test results in Table 1, taking Examples 1-2 and Comparative Example 1 as examples, although the addition of modified glass powder will reduce the mechanical tensile properties of the PSU membrane, the reduction is small, and the mechanical properties of the PSU membrane are effectively maintained. After ultraviolet aging, the mechanical tensile properties of the PSU membrane of Examples 1-2 have a high retention rate, and the transmittance is still maintained at more than 80%. Therefore, it is suitable for application scenarios with strong ultraviolet radiation and has higher durability.
[0059] Taking Example 1 and Comparative Example 2 as examples, it can be seen that the addition of unmodified glass powder causes the tensile properties of the PSU film to be severely reduced due to the poor dispersibility of the glass powder, and the degree of performance degradation after ultraviolet aging is even higher.
[0060] Taking Example 1 and Comparative Examples 3-4 as examples, it can be seen that the mechanical properties of the PSU film obtained by using glass powder modified by PSU or PPSU cannot be well maintained after ultraviolet aging. Therefore, it is shown that the glass powder modified by PESU can effectively enhance the ultraviolet aging resistance of the PSU film.
[0061] Taking Example 1 and Example 3 as examples, it can be seen that selecting a PESU resin with a moderate molecular weight to modify the glass powder can further improve the UV aging resistance of the PSU film.
[0062] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A three-layer co-extruded PSU film, characterized in that: The invention comprises a PSU layer and two modified PSU layers, wherein the PSU layer is arranged between the two modified PSU layers, and the modified PSU layer is prepared from raw materials comprising the following parts by weight: PSU resin 100 parts; 3~4.5 parts of modified glass powder; Antioxidant 0.7~1.2 parts; The modified glass powder is obtained by attaching PESU resin to the surface of the glass powder.
2. A three-layer co-extruded PSU film according to claim 1, characterized in that: The raw materials for preparing the modified glass powder include glass powder, PESU resin, ether, water and dimethylacetamide, and the mass ratio of the glass powder, PESU resin, ether, water and dimethylacetamide is 1:(0.1-0.25):(3-5):(6-10):(2-4).
3. A three-layer co-extruded PSU film according to claim 2, characterized in that: The preparation method of the modified glass powder comprises the following steps: dissolving PESU resin in dimethylacetamide, adding glass powder into the dimethylacetamide, firstly adding ether dropwise, stirring evenly, then adding water dropwise, stirring evenly, separating, and obtaining the modified glass powder.
4. A three-layer co-extruded PSU film according to claim 2, characterized in that: The particle size of the glass powder is 1-5 μm.
5. A three-layer co-extruded PSU film according to claim 1, characterized in that: The molecular weight of the PSU resin is 78,000-84,000.
6. A three-layer co-extruded PSU film according to claim 1, characterized in that: The molecular weight of the PESU resin is 45,000-51,000.
7. A three-layer co-extruded PSU film according to claim 1, characterized in that: The antioxidant is selected from one or both of antioxidant 1024 and antioxidant DLTP.
8. A method for preparing a three-layer co-extruded PSU film according to any one of claims 1 to 7, characterized in that: The following steps are involved: PSU resin is dried for later use; PSU resin, modified glass powder and antioxidant are mixed, heated, extruded and granulated to obtain modified PSU particles, and the modified PSU particles are heated to obtain a modified PSU melt; The PSU resin is heated to obtain a PSU melt; The modified PSU melt is distributed to the upper flow channel and the lower flow channel of the die distributor, and the PSU melt is distributed to the middle flow channel of the die distributor. Then the modified PSU melt and the PSU melt are compound co-extruded in the co-extrusion die, and after co-extrusion, they are cast into a film, cooled and shaped to obtain a three-layer co-extruded PSU film.
Citation Information
Patent Citations
A polyether sulphone / polyphenylene sulfide alloy, and a preparing method and application thereof
CN109777106A
Anti-ultraviolet polyether sulfone resin and preparation method thereof
CN113881227A
High modulus polyether sulfone compositions with improved impact
US6495615B1