Preparation method for co-production of silicon-carbon negative electrode material and high-order silane, silicon-carbon negative electrode material, high-order silane and lithium battery
By co-depositing and processing porous carbon substrate and silane in the preparation of lithium-ion battery negative electrode materials and collecting higher-order silanes, the problems of silicon carbon material performance and difficulty in collecting higher-order silanes are solved, and efficient silicon carbon negative electrode materials and High-order silane co-production improves battery performance and resource utilization.
Patent Information
- Application Number
- CN202410817550.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-15
AI Technical Summary
During the preparation of existing lithium-ion battery negative electrode materials, silicon carbon materials have limited performance and are difficult to collect high-order silanes, resulting in waste of materials and high production costs.
By co-deposition of the porous carbon substrate and silane, the temperature is controlled at 300°C to 400°C, the gas flow rate is 70g/min to 150g/min, and the pressure is 0.2MPa to 2MPa, the solid phase is collected to obtain the silicon-carbon negative electrode material and The gas phase is separated to obtain higher order silanes, and a carbon layer is deposited on the surface of the silicon-carbon anode material.
The cogeneration of high-order silanes and the efficient preparation of silicon-carbon anode materials are achieved, the capacity and circulation performance of the materials are improved, the decomposition of by-products is reduced, and the resource utilization and product consistency are improved.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of preparation of battery negative electrode materials, and in particular to a preparation method of a silicon-carbon negative electrode material and a high-order silane co-production, a silicon-carbon negative electrode material, a high-order silane and a lithium battery. Background Art
[0002] Lithium-ion batteries have attracted much attention due to their high energy density and long cycle life. However, with the continuous development of electronic devices such as electric vehicles and smartphones, the requirements for battery performance are also increasing. As a key component of lithium-ion batteries, the performance of negative electrode materials has an important impact on the overall performance of the battery.
[0003] At present, in the process of preparing silicon-carbon negative electrode materials by using chemical vapor deposition method, the method decomposes gas raw materials such as silane under high temperature conditions and deposits them on porous carbon materials. Specifically, in this process, silane is heated and cracked to generate SiH2 radicals. In addition to generating elemental silicon, free radical rearrangement reaction will also occur to generate trace amounts of higher-order silanes. Although the silicon-carbon negative electrode material prepared by this method has good performance, there is still a lot of room for improvement in obtaining silicon-carbon negative electrode materials with high capacity and excellent cycle performance. At the same time, the generation of trace amounts of high-order silanes is not convenient for collection, resulting in material waste.
[0004] In advanced semiconductor manufacturing processes, high-order silanes, especially disilane, play an irreplaceable and important role. As a source gas for silicon-based thin film deposition, it is the only silicon source gas that can be used in the initial stage of 14nm and below 3D NAND memory chip manufacturing processes. At present, the mass production process of high-order silane is the silicon-magnesium alloy method, and its production process is an intermittent process with many side reactions. The elements cannot be closed-loop, resulting in a large amount of "three wastes", the conversion rate of disilane is low, and the total cost is extremely high. Summary of the invention
[0005] Based on this, a method for preparing a silicon-carbon negative electrode material and a high-order silane co-production, a silicon-carbon negative electrode material, a high-order silane and a lithium battery are provided, which can realize the co-production of high-order silane and simultaneously prepare a silicon-carbon negative electrode material with high capacity and excellent energy conversion efficiency.
[0006] A method for preparing a silicon-carbon negative electrode material and a co-production of high-order silane, the preparation method comprising the following steps:
[0007] The porous carbon substrate is co-deposited with monosilane (SiH4), the solid phase is collected to obtain the silicon-carbon negative electrode material, and the collected gas phase is separated to obtain the high-order silane (Si n H 2n+2 ; n>1);
[0008] The temperature of the co-deposition process is 300°C to 400°C.
[0009] In any embodiment, the gas flow rate of monosilane in the co-deposition process is 70 g / min to 150 g / min; and the pressure of the co-deposition process is 0.2 MPa to 2 MPa.
[0010] In any embodiment, the reaction time of the co-deposition treatment of the porous carbon substrate and monosilane is 0.1 h to 5 h.
[0011] In any embodiment, the porous carbon substrate satisfies the following conditions:
[0012] (1) 500m 2 / g≤BET≤2000m 2 / g;
[0013] (2) 4μm≤D 50 ≤20μm;
[0014] (3) 0.2 g / cm 3 ≤TD≤0.6g / cm 3 .
[0015] In any embodiment, the method further comprises introducing a carbon source gas into the collected silicon-carbon negative electrode material to deposit a carbon layer on the surface of the silicon-carbon negative electrode material.
[0016] In any embodiment, the carbon source gas includes a gas-phase alkane compound.
[0017] In any embodiment, the temperature of the carbon layer deposition is 500° C. to 700° C.; the pressure is 0.05 MPa to 0.15 MPa; and the flow rate of the carbon source gas is 0.2 m / min to 5 m / min.
[0018] In any embodiment, the carbon layer is deposited to a thickness of 1 nm to 100 nm.
[0019] The second aspect of the present application discloses a silicon-carbon negative electrode material, which is prepared by the preparation method of the silicon-carbon negative electrode material and high-order silane co-production described in any of the above embodiments.
[0020] The third aspect of the present application discloses a high-order silane, which is prepared by the method for co-producing the silicon-carbon negative electrode material and the high-order silane described in any of the above embodiments.
[0021] The fourth aspect of the present application discloses a negative electrode sheet, which contains a silicon-carbon negative electrode material prepared by a preparation method of co-producing a silicon-carbon negative electrode material and a high-order silane.
[0022] The fifth aspect of the present application discloses a lithium battery, which contains a negative electrode sheet prepared from the above-mentioned silicon-carbon negative electrode material.
[0023] Beneficial effects:
[0024] The preparation method of silicon-carbon negative electrode material and high-order silane co-production of the present application can effectively realize the co-production of silicon-carbon negative electrode material and high-order silane. The preparation method of the present invention increases the output of high-order silane, which is beneficial to the recovery and utilization of by-products in the preparation process of silicon-carbon negative electrode material, and improves resource utilization; and can promote the adsorption of silane on porous carbon, inhibit the conversion of amorphous silicon to single crystal silicon in porous carbon, and further improve the product consistency of carbon negative electrode material in the vapor deposition process, so that the prepared carbon negative electrode material has the advantages of high capacity and excellent cycle performance. DETAILED DESCRIPTION
[0025] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.
[0026] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0027] As used herein, the term "prepared from" is synonymous with "comprising". As used herein, the terms "comprising", "including", "having", "containing" or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0028] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0029] The following is a detailed description of the preparation method of the silicon-carbon negative electrode material and the co-production of high-order silane, the silicon-carbon negative electrode material, the high-order silane and the lithium battery provided in the embodiments of the present invention.
[0030] One aspect of the present application provides a method for preparing a silicon-carbon negative electrode material and a co-production of high-order silane, the preparation method comprising the following steps:
[0031] The porous carbon substrate is co-deposited with monosilane, the solid phase is collected to obtain a silicon-carbon negative electrode material, and the collected gas phase is separated to obtain a high-order silane;
[0032] In the present application, during the co-deposition process of the porous carbon substrate and monosilane, monosilane is adsorbed to the inner surface of the porous carbon substrate and then cracked, and amorphous nano-state elemental silicon is deposited inside the porous carbon substrate. Under the catalytic action of the porous carbon substrate, monosilane is heated and cracked to generate SiH2 free radicals, and the SiH2 free radicals will react in parallel in two directions: first, further cracking to generate elemental silicon and hydrogen; on the other hand, free radical rearrangement reaction occurs to generate higher-order silanes, which include disilane and trisilane.
[0033] In some embodiments, the temperature of the co-deposition process is 300° C. to 400° C. Specifically, the temperature includes but is not limited to 300° C., 360° C., 390° C., and 400° C.
[0034] It should be noted that in the related art, the temperature range of the co-deposition treatment of the porous carbon substrate and other monosilanes such as monosilane is generally 500°C to 700°C. In this temperature range, monosilane can be effectively cracked and then generate SiH2 free radicals. However, in this temperature range, the high-order silanes generated by the free radical rearrangement reaction of SiH2 are easily decomposed as the co-deposition process proceeds. Therefore, the content of high-order silanes in the gas phase is low, difficult to collect, and the final collection rate is low.
[0035] The present application controls the temperature within the range of 300°C to 400°C, which can ensure the cracking of silane on the one hand, and inhibit the decomposition of higher-order silane on the other hand. At the same time, at this reaction temperature, the amorphous nano-state single silicon deposited inside the porous carbon substrate can be effectively reduced to undergo a crystal phase transformation to form crystalline silicon, thereby avoiding the electrochemical properties of the prepared silicon-carbon negative electrode material, such as the capacity, cycle stability, and rate performance of the negative electrode material, being affected by the presence of crystalline silicon, which is conducive to making the subsequently prepared silicon-carbon negative electrode material have a higher product consistency.
[0036] In some embodiments, the gas flow rate of monosilane is 70 g / min to 150 g / min. Specifically, the gas flow rate includes but is not limited to 70 g / min, 90 g / min, 110 g / min, and 150 g / min.
[0037] The present application controls the gas flow rate of monosilane within the range of 70 g / min to 150 g / min, which can increase the gas flow rate, enhance convection and heat dissipation, reduce the temperature in the reaction area, further inhibit the decomposition of high-order silanes, and help increase the yield of high-order silanes. If the flow rate is too high, it is easy to take away too much powder material, and if the flow rate is too low, it will lead to a large difference in the concentration of the inlet and outlet raw materials, poor product uniformity, and too long reaction time, excessive decomposition of high-order silanes, and too low yield.
[0038] In some embodiments, the co-deposition process is performed at a pressure of 0.2 MPa to 2 MPa. Specifically, the pressure includes but is not limited to 0.2 MPa, 0.5 MPa, 1 MPa, 1.5 MPa, and 2 MPa.
[0039] Furthermore, since the present application controls the gas flow rate of monosilane within the range of 70 g / min to 150 g / min, if the monosilane gas flow rate is too high, the temperature will be reduced and the residence time of the monosilane gas in the reaction area will be reduced, which is equivalent to reducing the reaction concentration of the reactants, resulting in a decrease in the overall conversion rate of monosilane. The present application controls the co-deposition pressure within the range of 0.2 MPa to 2 MPa, which can increase the concentration of monosilane and thereby increase the production capacity of higher-order silanes per unit time.
[0040] In some embodiments, the reaction time of the co-deposition treatment of the porous carbon substrate and monosilane is 0.1 h to 5 h. Specifically, the reaction time includes but is not limited to 0.1 h, 1 h, 2 h, 3 h, 4 h, and 5 h.
[0041] In the present application, a porous carbon substrate is used as a substrate for monosilane gas deposition, and the preparation method of the porous carbon is a conventional preparation method in the art. Generally, the porous carbon substrate can be commercially available porous carbon.
[0042] In order to improve the adsorption and cracking of monosilane, thereby improving the preparation efficiency and performance of silicon-carbon negative electrode materials and high-order silanes, 500m 2 / g≤BET≤2000m 2 / g, 4μm≤D 50 ≤20μm and 0.2g / cm 3 ≤TD≤0.6g / cm 3 Porous carbon. Wherein, BET is specific surface area. Selecting the specific surface area in the above range can make the porous carbon substrate have more active sites, which is conducive to the preparation of the silicon-carbon negative electrode material with better capacitance, cycle stability, etc.; D 50 It refers to the particle size corresponding to the cumulative distribution of 50% in the particle size distribution. The use of the above particle size is conducive to the uniformity and consistency of preparing silicon-carbon negative electrode materials. TD refers to the tap density. The use of porous carbon with the above tap density is conducive to helping to improve the volume energy density of the prepared silicon-carbon negative electrode material, thereby improving the overall performance of the battery.
[0043] The specific surface area of the porous carbon substrate of the present application has a meaning well known in the art, and can be measured using instruments and methods well known in the art. For example, it can refer to GB / T19587-2017 gas adsorption BET method for determining the specific surface area of solid substances, and be tested using a nitrogen adsorption specific surface area analysis test method, and calculated using the BET (Brunauer Emmett Teller) method, wherein the nitrogen adsorption specific surface area analysis test can be performed using the TriStarⅡ3020 specific surface and pore analyzer from Micromeritics, USA.
[0044] The median particle size D50 of the porous carbon substrate of the present application has a well-known meaning in the art and can be measured by instruments and methods well-known in the art. For example, it can be conveniently measured by a laser particle size analyzer with reference to the particle size distribution laser diffraction method of GB / T19077-2016, such as the Mastersizer 2000E laser particle size analyzer of Malvern Instruments Ltd., UK.
[0045] The tap density of the porous carbon substrate of the present application is a well-known meaning in the art, and can be measured, for example, according to GB / T1482-2016 "Determination of tap density of powdered materials". It can be conveniently measured by a tap density meter, such as the BT-300 tap density meter of Dandong Better Instrument Co., Ltd.
[0046] In any embodiment, the equipment for vapor deposition processing is conventional equipment in the art, including but not limited to a rotary furnace, a fixed bed, a moving bed, and a fluidized bed.
[0047] In the present application, the method for separating the collected gas phase is a conventional method in the art, including but not limited to distillation.
[0048] In any embodiment, the number of gas phase separations is not limited, and can be 1 time, 2 times, 3 times, 4 times, or 5 times.
[0049] As a high-value chemical raw material, high-order silane is widely used in the fields of semiconductors, solar cells, optical materials, etc. The silicon-carbon negative electrode material and the preparation method of high-order silane co-production of the present application are not only conducive to the recovery and utilization of the subsequent reaction tail gas, but also can realize the co-production of high-order silane, so that resources are maximized.
[0050] In some embodiments, after the porous carbon substrate and monosilane are co-deposited, the introduction of monosilane into the reactor is stopped, and then a carbon source gas is introduced into the collected silicon-carbon negative electrode material to deposit a carbon layer on the surface of the silicon-carbon negative electrode material.
[0051] Optionally, the reaction time for depositing the carbon layer on the surface of the silicon-carbon negative electrode material is 0.1 to 2 hours. Specifically, the reaction time includes but is not limited to 0.5 hours, 1 hour, 1.5 hours, and 2 hours.
[0052] Optionally, the reaction temperature for depositing the carbon layer on the surface of the silicon-carbon negative electrode material is 500° C. to 700° C. Specifically, the reaction temperature includes but is not limited to 500° C., 550° C., 600° C., 650° C., and 700° C.
[0053] Optionally, the flow rate of the carbon source gas is 0.2 g / min to 5 g / min. Specifically, the flow rate includes but is not limited to 0.5 g / min, 1 g / min, 2 g / min, 3 g / min, 4 g / min, and 5 g / min.
[0054] Optionally, the carbon source gas includes a gas-phase alkane compound, and specifically one or more of alkanes, alkenes and alkynes can be selected.
[0055] It should be specifically noted that the deposited carbon layer in the present application is amorphous carbon. The deposited carbon layer can serve as a physical barrier to reduce the risk of direct contact between the silicon-containing material in the silicon-carbon negative electrode material and the ambient atmosphere or electrolyte. For example, in the application process of the negative electrode active material, it can reduce the gas production during the pulping process and reduce the side reaction with the electrolyte during the charge and discharge cycle, thereby being more conducive to the electrochemical performance of the negative electrode active material.
[0056] Optionally, the thickness of the carbon layer deposition is 1nm to 100nm. In this way, it has a good physical barrier effect, can effectively improve the electronic conductivity of silicon-carbon particles, and can also shorten the extraction / embedding path of active ions in silicon-carbon particles. Specifically, the thickness of the carbon layer can be, but is not limited to, 1nm, 5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm.
[0057] The second aspect of the present application provides a silicon-carbon negative electrode material, which is obtained by a preparation method of a silicon-carbon negative electrode material and a high-order silane co-production according to any of the above embodiments, thereby obtaining a silicon-carbon negative electrode material with high product consistency, which has the advantages of high capacity and good cycle performance.
[0058] The third aspect of the present application provides a high-order silane, which is obtained by a preparation method of a silicon-carbon negative electrode material and a high-order silane co-production according to any of the above embodiments.
[0059] A fourth aspect of the present application provides a negative electrode sheet, which contains the silicon-carbon negative electrode material prepared by the above method.
[0060] In the present application, the negative electrode sheet comprises a current collector, a binder, a conductive agent and a negative electrode active material, wherein the negative electrode current collector may be a metal foil or a composite current collector. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS). The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers, and the negative electrode active material is the silicon-carbon negative electrode material of the second aspect of the present application.
[0061] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0062] In some embodiments, the negative electrode sheet can be prepared in the following manner: the above-mentioned components for preparing the negative electrode sheet, such as silicon-carbon negative electrode active material, conductive agent, binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0063] The fifth aspect of the present application provides a lithium battery, which is composed of a positive electrode plate, a negative electrode plate, a separator, and an electrolyte, wherein the negative electrode plate contains the silicon-carbon negative electrode material prepared by the above method.
[0064] In the present application, the positive electrode sheet includes a current collector, a binder, a conductive agent and a positive active material, wherein the positive current collector may be a metal foil or a composite current collector. The binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. The conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. The positive active material may be a positive active material for a battery known in the art. As an example, the positive active material may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive active materials for batteries may also be used.
[0065] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0066] In some embodiments, optionally, a button cell is made using metallic lithium as a counter electrode.
[0067] In the present application, the electrolyte can be selected according to the needs. For example, the electrolyte salt can be selected from lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate and lithium tetrafluorooxalate phosphate. At least one of the solvent can be selected from ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0068] In the present application, the separator can be selected according to the needs. For example, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without special restrictions. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without special restrictions.
[0069] The following is a further detailed description of the preparation method of the silicon-carbon negative electrode material and the preparation method of the co-production of high-order silane of the present application in combination with the embodiments and comparative examples.
[0070] Example 1
[0071] (1) The reactor was filled with 5 kg of porous carbon (BET: 1905 m2 / g, D50: 8 μm, TD: 0.33 g / cm 3 ), heated to 400°C, 0.2MPa silane was introduced into the reactor at a flow rate of 70g / min for reaction, and the reaction was continuously run for 5 hours;
[0072] (2) distilling and separating the tail gas in the reactor to obtain high-order silanes;
[0073] (3) Acetylene at normal pressure was introduced into the reactor at a flow rate of 4 g / min for 2 hours to obtain a silicon-carbon negative electrode material.
[0074] Example 2
[0075] (1) The reactor was filled with 5 kg of porous carbon (BET: 1905 m2 / g, D50: 8 μm, TD: 0.33 g / cm 3 ), heated to 300°C, 2MPa silane was introduced into the reactor at a flow rate of 110g / min for reaction, and the reaction was continuously operated for 5 hours;
[0076] (2) distilling and separating the tail gas in the reactor to obtain high-order silanes;
[0077] (3) Acetylene at normal pressure was introduced into the reactor at a flow rate of 4 g / min for 2 hours to obtain a silicon-carbon negative electrode material.
[0078] Example 3
[0079] (1) The reactor was filled with 5 kg of porous carbon (BET: 1905 m2 / g, D50: 8 μm, TD: 0.33 g / cm 3 ), heated to 400°C, 0.4MPa silane was introduced into the reactor at a flow rate of 90g / min for reaction, and the reaction was continuously operated for 5 hours;
[0080] (2) distilling and separating the tail gas in the reactor to obtain high-order silanes;
[0081] (3) Acetylene at normal pressure was introduced into the reactor at a flow rate of 4 g / min for 2 hours to obtain a silicon-carbon negative electrode material.
[0082] Example 4
[0083] (1) The reactor was filled with 5 kg of porous carbon (BET: 1905 m2 / g, D50: 8 μm, TD: 0.33 g / cm 3 ), heated to 390°C, 1MPa silane was introduced into the reactor at a flow rate of 90g / min for reaction, and the reaction was continuously run for 5 hours;
[0084] (2) distilling and separating the tail gas in the reactor to obtain high-order silanes;
[0085] (3) Acetylene at normal pressure was introduced into the reactor at a flow rate of 4 g / min for 2 hours to obtain a silicon-carbon negative electrode material.
[0086] Example 5
[0087] (1) The reactor was filled with 5 kg of porous carbon (BET: 1905 m2 / g, D50: 8 μm, TD: 0.33 g / cm 3 ), heated to 350°C, 1.5MPa silane was introduced into the reactor at a flow rate of 150g / min for reaction, and the reaction was continuously run for 5 hours;
[0088] (2) distilling and separating the tail gas in the reactor to obtain high-order silanes;
[0089] (3) Acetylene at normal pressure was introduced into the reactor at a flow rate of 4 g / min for 2 hours to obtain a silicon-carbon negative electrode material.
[0090] Example 6
[0091] (1) The reactor was filled with 5 kg of porous carbon (BET: 1905 m2 / g, D50: 8 μm, TD: 0.33 g / cm 3 ), heated to 360°C, 0.8MPa silane was introduced into the reactor at a flow rate of 100g / min for reaction, and the reaction was continuously run for 5 hours;
[0092] (2) distilling and separating the tail gas in the reactor to obtain high-order silanes;
[0093] (3) Acetylene at normal pressure was introduced into the reactor at a flow rate of 4 g / min for 2 hours to obtain a silicon-carbon negative electrode material.
[0094] Comparative Example 1
[0095] The only difference from Example 6 is that the reactor is heated to 500° C. and the reaction is continued at the preset temperature for 5 hours.
[0096] Comparative Example 2
[0097] The only difference from Example 6 is that monosilane at normal pressure is introduced into the reactor to react with the porous carbon continuously for 5 hours.
[0098] Comparative Example 3
[0099] The only difference from Example 6 is that 20 g / min of silane is introduced into the reactor to react with the porous carbon continuously for 25 hours.
[0100] Silicon-carbon anode material performance test:
[0101] (1) Powder resistivity test:
[0102] The resistivity tester was used to test. 1g of the negative electrode material of each embodiment and comparative example was placed between the electrodes of the resistivity tester. The electronic press was used to press the material to a constant pressure of 30 MPa for 15s-25s to obtain a sheet sample. The powder resistivity δ of the material was calculated according to the formula δ = (S × R) / h, in Ω·cm. Where h is the height of the sheet sample, in cm; R is the resistance, in Ω; S is the area of the sheet sample, in cm 2 .
[0103] (2) Using button cells to test specific capacity and initial coulombic efficiency:
[0104] Preparation of button cell: The silicon-carbon material, conductive additive carbon black, and binder (sodium carboxymethyl cellulose and styrene-butadiene rubber in a mass ratio of 1:1) of each embodiment and comparative example were weighed in a mass ratio of 94:2:4, and the slurry was prepared by a pulping machine, and a 250μm scraper was used to coat the negative electrode at 30mm / s on a coater, and baked at 80°C for 2h to obtain the negative electrode. A Celgard 2400 polypropylene diaphragm was used, a metal lithium sheet was selected as the positive electrode, and a LiPF6 system electrolyte (a LiPF6 solution with a concentration of 1 mol / L, and a 1:1 (volume ratio) mixed solution of ethylene carbonate (EC) / dimethyl carbonate (DMC) was used as the solvent) was used as the electrolyte, and the above-prepared negative electrode was assembled into a CR2032 button cell in a glove box.
[0105] The prepared CR2032 button battery was subjected to constant current charge and discharge test using a charge and discharge instrument, with the discharge cut-off voltage being 0.005V and the charge cut-off voltage being 2V, and the specific capacity was measured. The first week of charge and discharge test was carried out at a current density of 1C / 10C, and the first coulombic efficiency was tested, and the results are summarized in Table 1.
[0106] (3) Using the full electrical test method to test the cycle performance of each negative electrode material
[0107] Preparation of a full battery: Take the silicon-carbon particles obtained in each embodiment and comparative example, and configure them with graphite to form a composite material with a specific capacity of 450mAg / h. Weigh the composite material, conductive additive carbon black, and binder (sodium carboxymethyl cellulose and styrene-butadiene rubber in a mass ratio of 1:1) in a mass ratio of 94:2:4 to prepare a slurry, apply the slurry on the current collector, and obtain a negative electrode for standby use. The positive active material LiCoO2, conductive carbon black, and binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in an N-methylpyrrolidone solvent system in a weight ratio of 96.7:1.7:1.6, and then coated on Al foil for drying and cold pressing to obtain a positive electrode for standby use. Using a polyethylene porous polymer film as a separator, the above-mentioned positive electrode, separator, and negative electrode are stacked in order, so that the separator is between the positive electrode and the negative electrode to play an isolating role, and wound to obtain a bare battery cell. The bare cell was placed in an outer package and injected with electrolyte to prepare a 404865 cell (positive electrode surface density 17.9 g / cm 2 , negative electrode surface density 7.0g / cm 2 The electrolyte uses Xinzhoubang LBC421B10) and is packaged, and the full battery cell is obtained through the process of formation, degassing, and trimming.
[0108] The formula for calculating the yield of higher-order silanes is:
[0109]
[0110] Where: η——high-order silane yield
[0111] m0——Total mass of silane introduced
[0112] m1——mass of disilane collected
[0113] m2——mass of trisilane collected
[0114] m——Total mass of collected higher-order silanes
[0115] According to the above formula, it can be approximately considered that:
[0116] High-order silane yield (%) = (total mass of collected high-order silane / total mass of introduced monosilane) × 100%
[0117] The performance of the silicon-carbon negative electrode materials and the yield of high-order silanes in Examples 1 to 6 and Comparative Examples 1 to 3 are shown in the table below.
[0118] Table 1
[0119]
[0120]
[0121] From the data in Table 1, we can see that:
[0122] (1) Yield of the obtained high-order silane:
[0123] It can be seen from Examples 1 to 6 that the embodiments of the present invention significantly obtain a higher high-order silane yield than the various comparative examples; further, by comparing the high-order silane yield data of Example 6 with that of Comparative Example 1, the high-order silane yield data of Example 6 with that of Comparative Example 2, and the high-order silane yield data of Example 6 with that of Comparative Example 3, it can be seen that the embodiments of the present invention can obtain a higher high-order silane yield by simultaneously controlling the temperature of the co-deposition process, the pressure of the co-deposition process, and the gas flow rate of monosilane.
[0124] (2) Electrochemical properties of the prepared silicon-carbon negative electrode material:
[0125] The silicon-carbon composite materials prepared in various embodiments of the present invention have significantly lower powder resistivity than those in various comparative examples, and the prepared batteries have better conductive properties.
[0126] Comparing Example 6 with Comparative Example 1, the powder resistivity of Example 6 is much lower than that of Comparative Example 1, and the first coulombic efficiency and 300-cycle capacity retention rate are higher; comparing Example 6 with Comparative Example 2, the powder resistivity of Example 6 is much lower than that of Comparative Example 2, and the discharge specific capacity is higher; comparing Example 6 with Comparative Example 3, the powder resistivity of Example 6 is much lower than that of Comparative Example 3, and the first coulombic efficiency and 300-cycle capacity retention rate are higher. Therefore, in terms of the electrochemical properties of powder resistivity, first coulombic efficiency, discharge specific capacity and 300-cycle capacity retention rate, the silicon-carbon negative electrode material prepared by the above-mentioned preparation method has higher product consistency, so that the carbon negative electrode material has the advantages of high capacity and excellent cycle performance.
[0127] In summary, the preparation method provided by the embodiment of the present invention has the following characteristics:
[0128] (1) The temperature of the co-deposition treatment is controlled to be 300°C to 400°C in the present application. Thus, the co-deposition reaction of the porous carbon substrate and monosilane is carried out at a relatively low heating temperature, which can promote the adsorption of monosilane on the porous carbon substrate, and is beneficial to inhibiting the conversion of amorphous silicon to single crystal silicon in the porous carbon, and is also beneficial to inhibiting the decomposition of higher-order silanes (SinH2n+2; n>1);
[0129] (2) By increasing the gas flow rate of monosilane, the gas can pass through the reaction area to cool the reaction area, which can further inhibit the decomposition of higher-order silanes, thereby increasing the yield of higher-order silanes and further improving the consistency of the product;
[0130] (3) In order to avoid a decrease in the overall conversion rate of monosilane due to a decrease in the concentration of reactants caused by increasing the gas flow rate of monosilane, the pressure of the co-deposition treatment is controlled to be 0.2 MPa to 2 MPa. Specifically, the concentration of monosilane can be increased by pressurizing monosilane to increase the production capacity of high-order silane per unit time.
[0131] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0132] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a silicon-carbon negative electrode material and a high-order silane co-production method, It is characterized in that The method comprises the following steps: The porous carbon substrate is co-deposited with monosilane, the solid phase is collected to obtain the silicon-carbon negative electrode material, and the collected gas phase is separated to obtain the high-order silane (Si n H 2n+2 ; n>1); The temperature of the co-deposition process is 300° C. to 400° C., the gas flow rate of monosilane in the co-deposition process is 70 g / min to 150 g / min, and the pressure of the co-deposition process is 0.2 MPa to 2 MPa.
2. The method for preparing the silicon-carbon negative electrode material and the co-production of high-order silane according to claim 1, It is characterized in that The reaction time of the co-deposition treatment of the porous carbon substrate and monosilane is 0.1h to 5h.
3. The method for preparing the silicon-carbon negative electrode material and the co-production of high-order silane according to claim 1, It is characterized in that The porous carbon substrate meets the following conditions: (1)500m 2 / g≤BET≤2000m 2 / g; (2)4μm≤D 50 ≤20μm; (3)0.2g / cm 3 ≤TD≤0.6g / cm 3 。 4. The method for preparing the silicon-carbon negative electrode material and the co-production of high-order silane according to claim 1 or 3, It is characterized in that The method further comprises introducing a carbon source gas into the collected silicon-carbon negative electrode material to deposit a carbon layer on the surface of the silicon-carbon negative electrode material; Preferably, the carbon source gas comprises a gas-phase alkane compound.
5. The method for preparing the carbon negative electrode material and the co-production of high-order silane according to claim 4, It is characterized in that The temperature of the carbon layer deposition is 500° C. to 700° C.; the pressure is 0.05 MPa to 0.15 MPa; and the flow rate of the carbon source gas is 0.2 g / min to 5 g / min.
6. The method for preparing the carbon negative electrode material and the co-production of high-order silane according to claim 5, It is characterized in that The thickness of the deposited carbon layer is 1 nm to 100 nm.
7. A silicon-carbon negative electrode material, It is characterized in that The silicon-carbon negative electrode material is prepared by the method for co-producing a silicon-carbon negative electrode material and a high-order silane as described in any one of claims 1 to 6.
8. A high-order silane, It is characterized in that The silicon-carbon negative electrode material is prepared by the method for co-producing a silicon-carbon negative electrode material and a high-order silane as described in any one of claims 1 to 6.
9. A negative electrode sheet, It is characterized in that The negative electrode sheet comprises the silicon-carbon negative electrode material as claimed in claim 7.
10. A lithium battery, It is characterized in that The lithium battery comprises the negative electrode sheet as claimed in claim 9.
Citation Information
Patent Citations
Silicon-carbon composite material, preparation method thereof, negative electrode and battery
CN117088375A
Silicon-carbon electrode material and preparation method therefor, negative electrode, battery, and device
WO2024046410A1