Lignin-based carbon dot composite material self-adaptive to wound microenvironment as well as preparation method and application of lignin-based carbon dot composite material
Through the adaptive wound microenvironment technology of lignin-based carbon dot composite materials, the ROS balance problem in bacterial infection and cell proliferation stages in wound treatment is solved, and efficient bacterial killing and tissue regeneration is achieved, providing a simple and low-quality Cost, biocompatible treatment options overcome the problems of DR bacterial infection and hypoxia.
Patent Information
- Application Number
- CN202411022870.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to achieve effective bactericidal in the bacterial infection stage and tissue regeneration in the cell proliferation stage in wound treatment, resulting in the problem of antibiotic resistance and ROS balance, and is costly and complex.
Develop a lignin-based carbon dot composite material adapted to the microenvironment of wounds. By combining lignin with peroxide, percarbonate or persulfate, hydrothermal treatment and organic acid treatment, it can prepare peroxide-like treatment. Enzyme and catalase-like nanomaterials can increase ROS during the bacterial infection stage and kill bacteria, and reduce ROS during the cell proliferation stage to promote tissue regeneration.
The adaptive balance of ROS in the wound microenvironment is achieved, providing a simple, low-cost, biocompatible therapeutic strategy, which can effectively kill bacteria and promote tissue regeneration, overcome the problems of DR bacterial infection and hypoxia, And it has little impact on normal tissue cells.
Smart Images

Figure HDA0004967789720000011 
Figure HDA0004967789720000012 
Figure HDA0004967789720000021
Abstract
Description
Technical Field
[0001] The invention relates to a lignin-based carbon dot composite material capable of self-adapting to wound microenvironment and a preparation method and application thereof, belonging to the technical field of material synthesis. Background Art
[0002] The discovery of antibiotics has saved countless lives. Currently, antibiotics are effective against bacteria mainly by interfering with the bacterial membrane, protein synthesis and DNA replication. However, over time, improper use and over-reliance on antibiotics have led to the rapid spread of antibiotic resistance (AMR), making the problem of drug-resistant microorganisms (DR) more serious. The emergence of DR bacteria has made it more difficult for modern medicine to treat infected wounds. The healing of bacterially infected wounds is a very complex biological process involving antibacterial, inflammatory responses, proliferation and tissue reconstruction. In the initial stage of wound treatment, antimicrobial agents are needed to improve wound healing. After reducing bacterial infection, the level of reactive oxygen species (ROS) needs to be controlled and sufficient oxygen needs to be provided to accelerate cell proliferation / collagen synthesis and promote tissue regeneration.
[0003] In order to reduce the use of antibiotics and avoid AMR, nanozymes as multifunctional and highly stable nanomaterials have attracted much attention in the biomedical field. Currently developed nanozymes achieve a combined effect of antibacterial and ROS removal in treatment by combining multiple enzyme functional materials. Or switch the enzyme-like activity of nanozymes through external intervention methods (such as sound wave-compression dynamic therapy, photothermal therapy, etc.) to achieve balanced regulation of ROS. However, the above methods are relatively complicated and costly.
[0004] Chinese patent document CN112647193A discloses a method for preparing an electron beam irradiated cross-linked calcium peroxide-carbon quantum dots@zein antibacterial film, comprising the following steps: S1: preparation of CaO2 nanoparticles; S2: preparation of carbon quantum dot solution; S3: electron beam irradiated cross-linked zein carbon quantum dot solution, adding CaO2 material, uniformly mixing as spinning solution, and electrospinning the spinning solution to form a fiber film. The addition of carbon quantum dots and CaO2 materials in this invention greatly improves the antibacterial properties of the fiber film, and exhibits excellent inhibitory effects on both Escherichia coli and Staphylococcus aureus. However, it can only sterilize by the production of H2O2, and cannot solve the problem of ROS balance in wound treatment, making it difficult to achieve self-adaptation in a complex wound microenvironment to promote wound healing.
[0005] Therefore, developing a simple, low-cost, biocompatible nanozyme material that can adapt to the wound microenvironment, increase ROS to kill bacteria during the bacterial infection stage, and reduce ROS to promote tissue regeneration according to changes in the wound environment during the cell proliferation stage, thereby achieving an adaptive balance of ROS, is of great significance for the treatment of infectious wounds. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention provides a lignin-based carbon dot composite material that is self-adaptive to wound microenvironment, and a preparation method and application thereof. The preparation process of the present invention is simple, low-cost and green and sustainable; the obtained lignin carbon dot and peroxide or percarbonate or persulfate composite material overcomes the main limitations of treating DR bacterial infected wounds (such as DR bacteria, hypoxia and limited H2O2 availability), can adapt to the wound microenvironment, increase ROS to kill bacteria during the bacterial infection stage, and reduce ROS to promote tissue regeneration according to changes in the wound environment during the cell proliferation stage, thereby achieving an adaptive balance of ROS, providing a convenient and feasible strategy and material for the comprehensive treatment of bacterial infected wounds; at the same time, it has good biocompatibility and minimal impact on normal tissue cells.
[0007] The present invention is achieved through the following technical solutions:
[0008] A lignin-based carbon dot composite material that is self-adaptive to wound microenvironment, wherein the lignin-based carbon dot composite material is a composite material of lignin-based carbon dots and peroxides, percarbonates or persulfates.
[0009] Preferably according to the present invention, in the lignin-based carbon dot composite material, the mass ratio of lignin-based carbon dots to peroxide, percarbonate or persulfate is 1:1 to 1:3.
[0010] The method for preparing the above-mentioned lignin-based carbon dot composite material that is self-adaptive to wound microenvironment comprises the steps of:
[0011] (1) fully dispersing lignin in deionized water; adding an organic acid and mixing uniformly; performing hydrothermal treatment, filtering, dialyzing, and drying to obtain lignin-based carbon dots;
[0012] (2) The lignin-based carbon dots and peroxides, percarbonates or persulfates are fully dispersed in ethanol, and the mixture is centrifuged, washed and dried to obtain a lignin-based carbon dot composite material that is adaptive to the wound microenvironment.
[0013] Preferably according to the present invention, in step (1), the lignin is alkaline lignin.
[0014] Preferably, according to the present invention, in step (1), the mass ratio of lignin to deionized water is (1-3): (20-50); preferably, the mass ratio of lignin to deionized water is (1-1.5): (20-30).
[0015] Preferably according to the present invention, in step (1), the organic acid is oxalic acid dihydrate, citric acid or tartaric acid; preferably, the organic acid is oxalic acid dihydrate.
[0016] Preferably according to the present invention, in step (1), the mass ratio of lignin to organic acid is (1-3): (1-3); preferably, the mass ratio of lignin to organic acid is (1-2): (1-2).
[0017] Preferably, in step (1), after adding the organic acid, stirring is performed at room temperature for 0.1 to 5 hours to mix evenly; preferably, stirring is performed at room temperature for 0.5 to 2 hours to mix evenly; most preferably, stirring is performed at room temperature for 1 hour to mix evenly.
[0018] Preferably according to the present invention, in step (1), the hydrothermal treatment temperature is 180-200°C; preferably, the hydrothermal treatment temperature is 180°C.
[0019] Preferably, according to the present invention, in step (1), the hydrothermal treatment time is 12 to 24 hours; preferably, the hydrothermal treatment time is 12 to 15 hours.
[0020] Preferably, according to the present invention, in step (1), the molecular weight cutoff of the dialysis bag or dialysis tubing used for dialysis is 1000-3000Da, and the dialysis time is 2 to 5 days; preferably, the molecular weight cutoff of the dialysis bag or dialysis tubing is 2000 to 3000Da, and the dialysis time is 2 to 3 days.
[0021] Preferably according to the present invention, in step (1), the drying method is freeze drying or vacuum drying; the drying time is 10 to 24 hours; preferably, the drying method is freeze drying, and the drying time is 12 to 15 hours; most preferably, the drying method is freeze drying, and the drying time is 12 hours.
[0022] Preferably according to the present invention, in step (2), the peroxide is calcium peroxide, sodium peroxide, potassium peroxide or peracetic acid; the percarbonate is sodium percarbonate, potassium percarbonate or ammonium percarbonate; the persulfate is sodium permonosulfate, potassium permonosulfate, ammonium permonosulfate, potassium persulfate, sodium persulfate, ammonium persulfate, calcium persulfate, zinc persulfate or magnesium persulfate; preferably, the peroxide is calcium peroxide.
[0023] Preferably, the preparation method of calcium peroxide includes the steps of: uniformly mixing an aqueous ammonia solution (NH3-H2O), polyethylene glycol, and an aqueous CaCl2 solution, adding an aqueous hydrogen peroxide solution, and adding an aqueous NaOH solution to adjust the pH value to 10-13; then filtering, washing, and drying to obtain CaO2.
[0024] More preferably, the concentration of the aqueous ammonia solution is 0.5 mol / L to 1 mol / L; the volume ratio of the aqueous ammonia solution to the polyethylene glycol is 1 to 5:10 to 12, preferably 1.2:12.
[0025] More preferably, the average molecular weight of polyethylene glycol is 200-2000; more preferably, the average molecular weight of polyethylene glycol is 200-1000; most preferably, the average molecular weight of polyethylene glycol is 200-400.
[0026] More preferably, the mass concentration of the aqueous hydrogen peroxide solution is 20-30%; most preferably, the mass concentration of the aqueous hydrogen peroxide solution is 25-30%.
[0027] More preferably, the concentration of the NaOH aqueous solution is 0.1 to 0.5 mol / L; more preferably, the concentration of the NaOH aqueous solution is 0.1 to 0.2 mol / L.
[0028] Further preferably, the concentration of the CaCl2 aqueous solution is 0.5-5 g / mL; the mass ratio of CaCl2 to polyethylene glycol is 3:10-12 g / mL; and the volume ratio of polyethylene glycol to the hydrogen peroxide aqueous solution is 10-12:1.5.
[0029] More preferably, the aqueous hydrogen peroxide solution is added to the system in a dropwise manner; the dropwise addition speed is 1 to 5 drops per minute; preferably, the dropwise addition speed is 3 to 5 drops per minute.
[0030] More preferably, after adding the aqueous hydrogen peroxide solution, stirring is carried out at room temperature for 1-5 hours.
[0031] More preferably, NaOH aqueous solution is added to adjust the pH value to 11-12.
[0032] More preferably, washing is first performed using a sodium hydroxide aqueous solution with a concentration of 0.1 mol / L-0.3 mol / L until the pH of the washing solution is 7-9, and then washing is performed using ethanol.
[0033] Further preferably, the drying method is freeze drying or vacuum drying; the drying time is 10 to 24 hours; further preferably, the drying method is vacuum drying, the drying temperature is 60 to 100°C, and the drying time is 12 to 15 hours; most preferably, the drying method is vacuum drying, the drying temperature is 80°C, and the drying time is 12 hours.
[0034] Preferably, according to the present invention, in step (2), the mass ratio of lignin-based carbon dots to ethanol is (0.01-0.05): (20-50) g / mL; preferably, the mass ratio of lignin-based carbon dots to ethanol is (0.03-0.05): (20-30) g / mL.
[0035] Preferably, according to the present invention, in step (2), the mass ratio of lignin-based carbon dots to peroxide, percarbonate or persulfate is (1-5): (1-5); preferably, the mass ratio of lignin-based carbon dots to peroxide, percarbonate or persulfate is (1-2): (1-2).
[0036] Preferably, according to the present invention, in step (2), the fully dispersed conditions are: stirring at room temperature for 20 to 24 hours; preferably, stirring at room temperature for 23 to 24 hours; most preferably, stirring at room temperature for 24 hours.
[0037] Preferably according to the present invention, in step (2), the drying method is freeze drying or vacuum drying; the drying time is 10 to 24 hours; preferably, the drying method is vacuum drying, the drying temperature is 50°C to 70°C, and the drying time is 20 to 24 hours; most preferably, the drying method is vacuum drying, the drying temperature is 60°C, and the drying time is 24 hours.
[0038] The application of the above-mentioned lignin-based carbon dot composite material that adapts to wound microenvironment in antibacterial applications.
[0039] Preferably according to the present invention, the lignin-based carbon dot composite material is used for sterilization or inhibition of Escherichia coli or Staphylococcus aureus.
[0040] The application of the above-mentioned lignin-based carbon dot composite material that adapts to the wound microenvironment in the production and / or removal of cellular reactive oxygen species.
[0041] Preferably according to the present invention, the lignin-based carbon dot composite material is used for removing or generating H2O2 in cells, or removing or generating reactive oxygen species in cells.
[0042] The application of the above-mentioned lignin-based carbon dot composite material that adapts to the wound microenvironment in the preparation of drugs or dressings for treating bacterially infected wounds.
[0043] Preferably, according to the present invention, the lignin-based carbon dot composite material can adapt to the wound microenvironment, increase ROS to kill bacteria during the bacterial infection stage, and reduce ROS to promote tissue regeneration according to changes in the wound environment during the cell proliferation stage, thereby achieving an adaptive balance of ROS.
[0044] The technical features and beneficial effects of the present invention are as follows:
[0045] 1. The present invention uses lignin as raw material and constructs a series of lignin-based carbon dots through a simple and effective strategy. The preparation process is simple, low-cost and green and sustainable; among them, the lignin-based carbon dots treated with oxalic acid have excellent peroxidase-like activity and catalase-like activity. The excellent bienzyme-like activity makes it possible to apply lignin-based carbon dots to ROS balance in the treatment of DR bacterial wounds.
[0046] 2. The lignin-based carbon dots prepared by the present invention have more C=O and COOH active sites, thus having the switching effect under acidic and alkaline conditions. The ROS generation mediated by the peroxidase-like activity of the lignin-based carbon dots can effectively kill bacteria, and the ROS removal mediated by the catalase-like activity of the lignin-based carbon dots can effectively protect cells and promote tissue regeneration, thereby achieving an adaptive balance of ROS at different stages of wound healing. In addition, the lignin-based carbon dots prepared with lignin and organic acids as raw materials have good biocompatibility.
[0047] 3. The lignin-based carbon dots in the composite material obtained by the present invention present a highly uniformly dispersed dot distribution. In the composite material of the present invention, the lignin-based carbon dots fully play the role of catalyzing extremely low concentration H2O2 to produce ROS to improve the bactericidal performance of the material, while avoiding the damage to the organism caused by the loss of transition metals, and have great application potential in biological sterilization and the preparation of durable spontaneous antibacterial personal protective equipment. It can continuously produce a large number of superoxide anion free radicals to destroy bacterial cell membranes.
[0048] 4. In the preparation method of the lignin-based carbon dot composite material developed in the present invention, the lignin is alkaline lignin, which can increase the surface C=O and COOH functional groups through organic acid treatment to achieve active site switching of dual enzyme activity. The other two organic acids (citric acid and tartaric acid) can also improve the dual enzyme activity of carbon dots, but the effect is still lower than that of oxalic acid. In addition, organic acid treatment is the key to the ROS balancing ability of lignin-based carbon dot composite materials. Without the addition of organic acid treatment, the ROS balancing ability of lignin-based carbon dot composite materials will be greatly reduced.
[0049] 5. The peroxide, percarbonate or persulfate such as CaO2 prepared by the method of the present invention is a block structure with good dispersibility. It can realize biocompatible treatment with intelligent H2O2 / O2 self-sufficiency in wound treatment (the environment is acidic under bacterial infection conditions, so that peroxide, percarbonate or persulfate reacts to produce H2O2; it is neutral or alkaline under physiological conditions, and peroxide, percarbonate or persulfate reacts to produce O2). Peroxide, percarbonate or persulfate such as CaO2 can also promote the migration and proliferation of fibroblasts and endothelial cells, which is crucial for tissue repair and angiogenesis in the wound healing process. The H2O2 provided by peroxide, percarbonate or persulfate such as CaO2 in the bacterial infection stage is catalyzed by lignin-based carbon dots to generate ROS to achieve efficient sterilization. At the same time, the oxygen released by peroxide, percarbonate or persulfate such as CaO2 helps promote angiogenesis at the wound site, which is very important for wound healing and tissue repair.
[0050] 6. The present invention constructs an adaptive ROS balance treatment platform by combining lignin-based carbon dots with peroxides or percarbonates or persulfates; the preparation process is simple, low-cost and green and sustainable, and the resulting composite material is an infected wound treatment nanomedicine with antibacterial, biodegradable and high biocompatibility. The present invention realizes a biocompatible adaptive ROS balance treatment platform with intelligent H2O2 / O2 self-sufficiency (providing H2O2 under bacterial infection conditions and O2 under physiological conditions), which overcomes the main limitations of treating DR bacterial infected wounds (such as DR bacteria, hypoxia and limited H2O2 availability) and has minimal impact on normal tissue cells. It can adapt to the wound microenvironment. In the bacterial infection stage, peroxides or percarbonates or persulfates are converted into H2O2. Lignin-based carbon dots produce and increase ROS through peroxidase-like activity to kill bacteria. In the cell proliferation stage, peroxides or percarbonates or persulfates are decomposed into H2O and O2 according to the changes in the wound environment. Lignin-based carbon dots decompose excess H2O2 into oxygen through catalase-like activity to reduce ROS and promote tissue regeneration, thereby achieving an adaptive balance of ROS, providing a convenient and feasible strategy and material for the comprehensive treatment of bacterial-infected wounds. At the same time, it has good biocompatibility and minimal effect on normal tissue cells. In vivo DR bacterial infection wound treatment further proves the feasibility and biocompatibility of the composite material for the treatment of DR bacterial infection wounds. The lignin-based carbon dot composite material proposed in the present invention has great application and expandability potential in the preparation of nanomaterials for the treatment of different bacterial infection wounds. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 is a transmission electron microscope (TEM) image of the lignin-based carbon dots prepared in Example 1.
[0052] Figure 2 This is the C spectrum of the X-ray photoelectron spectroscopy (XPS) of the lignin-based carbon dots prepared in Example 1.
[0053] Figure 3 It is the Fourier infrared spectra of the carbon dots prepared in Example 1 and Comparative Example 1, and the alkaline lignin in Comparative Example 2.
[0054] Figure 4 The graphs are peroxidase-like and catalase-like activity graphs of the composite materials prepared in Examples 1-3 and Comparative Examples 1 and 2.
[0055] Figure 5 Graphs showing the peroxidase-like and catalase-like activities of the composite materials prepared in Example 1 and Comparative Example 1 in buffer solutions of different pH values.
[0056] Figure 6 This is a transmission electron microscope (TEM) image of the calcium peroxide material prepared in Example 1.
[0057] Figure 7 This is the X-ray diffraction pattern of the lignin-based carbon dots, calcium peroxide and composite material prepared in Example 1.
[0058] Figure 8 This is a Fourier infrared spectrum of the lignin-based carbon dots, calcium peroxide and composite material prepared in Example 1.
[0059] Fig. 9 This is the C spectrum of the X-ray photoelectron spectroscopy (XPS) of the lignin-based carbon dots prepared in Comparative Example 1.
[0060] Fig.10 These are the plate photographs of the survival rates of Escherichia coli and Staphylococcus aureus incubated with lignin-based carbon dots under different conditions in Experimental Examples 1 and 2.
[0061] Fig.11 This is a comparison of the survival rates of Escherichia coli and Staphylococcus aureus incubated with lignin-based carbon dots under different conditions in Experimental Examples 1 and 2. The vertical axis is the survival rate.
[0062] Fig.12 It is a photograph of the survival rate of Escherichia coli and Staphylococcus aureus incubated at different composite material concentrations in Experimental Example 3.
[0063] Fig.13 This is a comparison chart of the survival rates of Escherichia coli and Staphylococcus aureus incubated at different composite material concentrations in Experimental Example 3. The vertical axis is the survival rate.
[0064] Fig.14 This is a cytotoxicity test diagram of the lignin-based carbon dots and composite materials prepared in Example 1. The horizontal axis is the material concentration, and the vertical axis is the cell survival rate.
[0065] Fig.15 This is a cell oxidation damage protection test graph of the lignin-based carbon dots and composite materials prepared in Example 1 in Test Example 6. The abscissa is the material concentration and test conditions, and the ordinate is the cell survival rate.
[0066] Fig.16 This is a diagram of the in vivo wound treatment effect of the composite material prepared in Example 1 of Experimental Example 7, including wound area display, mouse weight comparison, and hematoxylin and eosin staining and Masson staining images of tissues. DETAILED DESCRIPTION
[0067] The present invention is further described below by means of specific examples, but is not limited thereto.
[0068] The raw materials used in the following examples are all commercially available products and are analytically pure.
[0069] Example 1
[0070] A method for preparing a lignin-based carbon dot composite material, comprising the following steps:
[0071] (1) Disperse 1 g of alkaline lignin in 20 ml of distilled water, and then add 1 g of oxalic acid dihydrate of the same mass. After stirring for 1 h, transfer it to a Teflon high-pressure reactor and hydrothermally treat it at 180°C for 12 h. Filter it with a 0.22 μm filter membrane, collect the liquid product, and dialyze it in distilled water for 2 days using a dialysis tube (molecular weight cutoff of 2000 Da). Then freeze-dry the obtained yellow solution for 12 h to prepare lignin-based carbon dot powder.
[0072] The TEM morphology of the lignin-based carbon dots (LCDs-OA) prepared in this example is shown in Figure 1 As shown, it is a highly dispersed point distribution.
[0073] The C1s spectrum of the X-ray photoelectron spectroscopy (XPS) of the lignin-based carbon dots (LCDs-OA) prepared in this example ( Figure 2 ), it can be seen that the surface of lignin-based carbon dots (LCDs-OA) has abundant C=O and COOH functional groups. The Fourier transform infrared spectroscopy analysis of lignin-based carbon dots (LCDs-OA) is shown in Figure 3 The X-ray diffraction pattern of lignin-based carbon dots (LCDs-OA) is shown in Figure 2. Figure 7 As shown in the figure, it can be seen that the lignin-based carbon dots have a graphite phase structure.
[0074] The peroxidase-like activity of lignin-based carbon dots (LCDs-OA) was evaluated using TMB as a substrate. In a typical experiment, 400 μL of 1.0 mg / mL lignin-based carbon dot material aqueous dispersion, 400 μL of 10 mM TMB aqueous solution, and 400 μL of 5 mM H2O2 aqueous solution were added to 2.8 mL of NaAc-HAc buffer at pH 5, and then incubated at 25°C for 10 min. The absorbance change at 652 nm was monitored using a UV-visible spectrophotometer. At the same time, no H2O2 aqueous solution or no carbon dots or no H2O2 aqueous solution and carbon dots were used as comparisons. Figure 4 As shown in a, the material prepared under the condition of adding H2O2 has excellent peroxidase performance (TMB+H2O2+LCDs-OA).
[0075] The generated oxygen was measured using a specific oxygen electrode on a multi-parameter analyzer to determine the catalase (CAT) activity of the lignin-based carbon dot (LCDs-OA) material. In a typical test, 0.4 mL of a 1.0 mg / mL aqueous dispersion of lignin-based carbon dot material and 0.4 mL of a 50 mM H2O2 aqueous solution were sequentially added to 3.2 mL of a buffer solution (0.1 M PBS buffer solution, pH = 7.4). The solubility (mg / mL) of the generated O2 was measured at different reaction times. Figure 4 As shown in b, the prepared material (LCDs-OA) has excellent catalase performance.
[0076] (2) The preparation method of CaO2 is as follows:
[0077] 1.2 ml of 1M ammonia solution (NH3-H2O) and 12 ml of polyethylene glycol 200 (PEG200) were mixed evenly. 3 g of CaCl2 (equivalent to 2.7 mmol) was dissolved in 3 ml of purified water and then added to the above solution and mixed evenly. Then, under stirring, 1.5 ml of 30wt% hydrogen peroxide solution was added to the above solution at a rate of 3 drops per minute and stirred at room temperature for two hours. Subsequently, NaOH aqueous solution (concentration of 0.1 mol / L) was added and stirring was continued until the pH value of the solution rose to 11.5. At this time, the formation of a white solid precipitate was observed and the precipitate was collected by filtering with filter paper. The precipitate was then rinsed with a 0.1M NaOH aqueous solution and the process was repeated until the pH value of the rinse solution dropped to 8. Afterwards, it was washed with ethanol and then dried in a vacuum environment at 80 degrees Celsius for 12 hours.
[0078] The TEM morphology of calcium peroxide prepared in this example is as follows Figure 6 As shown, it is a block distribution.
[0079] The X-ray diffraction pattern of calcium peroxide prepared in this example is as follows Figure 7 As shown, it has obvious characteristic peaks of calcium peroxide.
[0080] The Fourier transform infrared spectroscopy analysis of calcium peroxide prepared in this example is as follows Figure 8 As shown, a distinct characteristic peak of calcium peroxide was observed.
[0081] (3) After 50 mg of lignin-based carbon dots and 50 mg of CaO2 were mixed in equal proportions, the mixture was stirred at room temperature for 24 h in a 20 mL ethanol medium to form a composite material (LCDs-OA@CaO2). Finally, the composite material (LCDs-OA@CaO2) was successfully prepared by centrifugation, ethanol washing, and vacuum drying at 60 °C for 24 h.
[0082] The X-ray diffraction pattern of the composite material prepared in this embodiment is as follows: Figure 7 As shown, there are obvious characteristic peaks of calcium peroxide and carbon dot materials.
[0083] The Fourier transform infrared spectroscopy analysis of the composite material prepared in this example is as follows Figure 8 As shown, obvious characteristic transmission peaks of calcium peroxide and carbon dot materials were observed.
[0084] The peroxidase and catalase activities of the lignin-based carbon dot composite material (LCDs-OA) prepared in Example 1 were tested at different pH values.
[0085] TMB was used as a substrate to evaluate the peroxidase-like activity of the composite material at different pH. In a typical experiment, 400 μL of 1.0 mg / mL composite material aqueous dispersion and 400 μL of 10 mM TMB aqueous solution were added to 2.8 mL of NaAc-HAc buffer with a pH of 3.5 to 7.5, and then incubated at 25°C for 10 min, and the absorbance change at 652 nm was monitored using a UV-visible spectrophotometer. Figure 5 As shown in a. The performance of the composite material peroxidase decreases with the increase of pH.
[0086] The generated oxygen was measured using a specific oxygen electrode on a multiparameter analyzer to determine the catalase (CAT) activity of the composite material. In a typical test, 0.4 mL of a 1.0 mg / mL aqueous dispersion of the composite material was added to 3.2 mL of a buffer solution (PBS buffer solution, pH = 4-10). The solubility (mg / mL) of the generated O2 was measured at different reaction times. Figure 5 As shown in b, the catalase performance of the composite material increases with the increase of pH.
[0087] This demonstrates that the composite material, unlike lignin-based carbon dots (LCDs-OA), has the ability to modulate ROS through different activities at different pH without the addition of H2O2 aqueous solution.
[0088] Example 2
[0089] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), citric acid is used instead of oxalic acid; the other steps and conditions are consistent with Example 1.
[0090] The oxidase-like activity of lignin-based carbon dots (LCDs-CA) was evaluated using TMB as a substrate, and the test method was as described in Example 1. The peroxidase-like performance of the obtained material (TMB+H2O2+LCDs-CA) was lower than that of Example 1, as shown in FIG. Figure 4 As shown in a.
[0091] The catalase-like activity of the lignin-based carbon dots was evaluated using hydrogen peroxide as a substrate. The test method was as described in Example 1. The catalase-like performance of the obtained material (LCDs-CA) was lower than that of Example 1. Figure 4 As shown in b.
[0092] Example 3
[0093] A method for preparing a lignin-based carbon dot composite material, as described in Example 1, except that in step (1), tartaric acid is used instead of oxalic acid; the other steps and conditions are consistent with Example 1.
[0094] The peroxidase-like activity of lignin-based carbon dots (LCDs-TA) was evaluated using TMB as a substrate, and the test method was as described in Example 1. The peroxidase-like performance of the obtained material (TMB+H2O2+LCDs-TA) was lower than that of Example 1, as shown in FIG. Figure 4 As shown in a.
[0095] The catalase-like activity of the lignin-based carbon dots was evaluated using hydrogen peroxide as a substrate. The test method was as described in Example 1. The catalase-like performance of the obtained material (LCDs-TA) was lower than that of Example 1. Figure 4 As shown in b.
[0096] Example 4
[0097] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the amount of oxalic acid dihydrate used is 2 g, and the other steps and conditions are consistent with Example 1.
[0098] Example 5
[0099] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the amount of lignin used is 2 g, and the other steps and conditions are consistent with Example 1.
[0100] Example 6
[0101] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the amount of oxalic acid dihydrate used is 3 g, and the other steps and conditions are consistent with Example 1.
[0102] Example 7
[0103] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the amount of lignin used is 3 g, and the other steps and conditions are consistent with Example 1.
[0104] Example 8
[0105] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the stirring and mixing time is controlled to be 0.1 h, and the other steps and conditions are consistent with Example 1.
[0106] Example 9
[0107] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the stirring and mixing time is controlled to be 0.5 h, and the other steps and conditions are consistent with Example 1.
[0108] Example 10
[0109] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the stirring and mixing time is controlled to be 2 hours, and the other steps and conditions are consistent with Example 1.
[0110] Embodiment 11
[0111] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the stirring and mixing time is controlled to be 4 hours, and the other steps and conditions are consistent with Example 1.
[0112] Example 12
[0113] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the stirring and mixing time is controlled to 5 hours, and the other steps and conditions are consistent with Example 1.
[0114] Example 13
[0115] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the hydrothermal temperature is controlled at 190° C., and the other steps and conditions are consistent with Example 1.
[0116] Embodiment 14
[0117] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the hydrothermal temperature is controlled at 200° C., and the other steps and conditions are consistent with Example 1.
[0118] Embodiment 15
[0119] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the hydrothermal time is controlled at 20 hours, and the other steps and conditions are consistent with Example 1.
[0120] Example 16
[0121] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the hydrothermal time is controlled at 24 hours, and the other steps and conditions are consistent with Example 1.
[0122] Embodiment 17
[0123] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the molecular weight cutoff of the dialysis tube is 1000DA, and the other steps and conditions are consistent with Example 1.
[0124] Embodiment 18
[0125] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the molecular weight cutoff of the dialysis tube is 3000DA, and the other steps and conditions are consistent with Example 1.
[0126] Embodiment 19
[0127] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the dialysis time is 3 days, and the other steps and conditions are consistent with Example 1.
[0128] Embodiment 20
[0129] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the dialysis time is 4 days, and the other steps and conditions are consistent with Example 1.
[0130] Embodiment 21
[0131] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), the dialysis time is 5 days, and the other steps and conditions are consistent with Example 1.
[0132] Embodiment 22
[0133] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (2), the amount of ammonia water added is 3 ml; the other steps and conditions are consistent with Example 1.
[0134] Embodiment 23
[0135] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (2), the amount of ammonia water added is 5 ml; the other steps and conditions are consistent with Example 1.
[0136] Embodiment 24
[0137] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (2), the polyethylene glycol molecular weight used is polyethylene glycol 1000; the other steps and conditions are consistent with Example 1.
[0138] Embodiment 25
[0139] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (2), the amount of polyethylene glycol used is 10 ml; the other steps and conditions are consistent with Example 1.
[0140] Embodiment 26
[0141] .A method for preparing a lignin-based carbon dot composite material, as described in Example 1, except that: in step (2), the amount of polyethylene glycol used is 11 ml; the other steps and conditions are consistent with Example 1.
[0142] Embodiment 27
[0143] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (2), the concentration of the hydrogen peroxide aqueous solution is 20 wt %; the other steps and conditions are consistent with Example 1.
[0144] Embodiment 28
[0145] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (2), the hydrogen peroxide dripping speed is 1 drop per minute; the other steps and conditions are consistent with Example 1.
[0146] Embodiment 29
[0147] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (2), the hydrogen peroxide dripping speed is 5 drops per minute; the other steps and conditions are consistent with Example 1.
[0148] Embodiment 30
[0149] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (2), the concentration of the sodium hydroxide aqueous solution is 0.3 M; the other steps and conditions are consistent with Example 1.
[0150] Embodiment 31
[0151] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (2), the concentration of the sodium hydroxide aqueous solution is 0.5 M; the other steps and conditions are consistent with Example 1.
[0152] Embodiment 32
[0153] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (2), the pH is adjusted to 11; the other steps and conditions are consistent with Example 1.
[0154] Embodiment 33
[0155] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (2), the pH is adjusted to 12; the other steps and conditions are consistent with Example 1.
[0156] Embodiment 34
[0157] A method for preparing a lignin-based carbon dot composite material, as described in Example 1, except that in step (3), calcium peroxide is replaced by sodium peroxide; the other steps and conditions are consistent with Example 1.
[0158] Embodiment 35
[0159] A method for preparing a lignin-based carbon dot composite material, as described in Example 1, except that in step (3), calcium peroxide is replaced by potassium peroxide; the other steps and conditions are consistent with Example 1.
[0160] Embodiment 36
[0161] A method for preparing a lignin-based carbon dot composite material, as described in Example 1, except that in step (3), calcium peroxide is replaced with sodium peroxymonosulfate; the other steps and conditions are consistent with Example 1.
[0162] Embodiment 37
[0163] A method for preparing a lignin-based carbon dot composite material, as described in Example 1, except that in step (3), calcium peroxide is replaced with potassium persulfate; the other steps and conditions are the same as in Example 1.
[0164] Embodiment 38
[0165] A method for preparing a lignin-based carbon dot composite material, as described in Example 1, except that in step (3), calcium peroxide is replaced with ammonium persulfate; the other steps and conditions are the same as in Example 1.
[0166] Embodiment 39
[0167] A method for preparing a lignin-based carbon dot composite material, as described in Example 1, except that in step (3), calcium peroxide is replaced by potassium persulfate; the other steps and conditions are consistent with Example 1.
[0168] Embodiment 40
[0169] A method for preparing a lignin-based carbon dot composite material, as described in Example 1, except that in step (3), calcium peroxide is replaced by sodium persulfate; the other steps and conditions are consistent with Example 1.
[0170] Embodiment 41
[0171] A method for preparing a lignin-based carbon dot composite material, as described in Example 1, except that in step (3), calcium peroxide is replaced with ammonium persulfate; the other steps and conditions are consistent with Example 1.
[0172] Embodiment 42
[0173] A method for preparing a lignin-based carbon dot composite material, as described in Example 1, except that in step (3), calcium peroxide is replaced with zinc persulfate; the other steps and conditions are consistent with Example 1.
[0174] Embodiment 43
[0175] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (3), calcium peroxide is replaced with calcium persulfate; the other steps and conditions are consistent with Example 1.
[0176] Embodiment 44
[0177] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (3), calcium peroxide is replaced with magnesium persulfate; the other steps and conditions are the same as in Example 1.
[0178] Embodiment 45
[0179] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (3), calcium peroxide is replaced with peracetic acid; the other steps and conditions are the same as in Example 1.
[0180] Embodiment 46
[0181] A method for preparing a lignin-based carbon dot composite material, as described in Example 1, except that in step (3), calcium peroxide is replaced by sodium percarbonate; the other steps and conditions are consistent with Example 1.
[0182] Embodiment 47
[0183] A method for preparing a lignin-based carbon dot composite material, as described in Example 1, except that in step (3), calcium peroxide is replaced with potassium percarbonate; the other steps and conditions are consistent with Example 1.
[0184] Embodiment 48
[0185] A method for preparing a lignin-based carbon dot composite material, as described in Example 1, except that in step (3), calcium peroxide is replaced with ammonium percarbonate; the other steps and conditions are consistent with Example 1.
[0186] Comparative Example 1
[0187] A method for preparing a lignin-based carbon dot composite material is as described in Example 1, except that in step (1), no organic acid is added; the other steps and conditions are consistent with Example 1.
[0188] The C1s spectrum ( Fig. 9 ), it can be seen that compared with the lignin-based carbon dots (LCDs-OA) synthesized in Example 1, the surface has fewer C=O and COOH functional groups. The Fourier transform infrared spectroscopy analysis of lignin-based carbon dots (LCDs) is shown in Figure 3 As shown, the same results as XPS were observed in the material.
[0189] The peroxidase-like activity of lignin-based carbon dots (LCDs) was evaluated using TMB as a substrate, and the test method was as described in Example 1. The peroxidase-like performance of the obtained material (TMB+H2O2+LCDs) decreased, as shown in FIG. Figure 4 As shown in a.
[0190] The catalase-like activity of the lignin-based carbon dots was evaluated using hydrogen peroxide as a substrate. The test method was as described in Example 1. The catalase-like performance of the obtained material (LCDs) was lower than that of Example 1. Figure 4 This proves that organic acid treatment can effectively improve the peroxidase and catalase activities of lignin-based carbon dots (LCDs-OA), thereby achieving efficient adaptive ROS balance ability.
[0191] The peroxidase and catalase activities of the lignin-based carbon dot composite material (LCDs) prepared in this comparative example at different pH values were tested, and the testing method was the same as that in Example 1. This indicates that the composite material prepared in this comparative example has poor self-adaptive regulation ability.
[0192] Comparative Example 2
[0193] Commercially available alkaline lignin was used for comparison without any treatment.
[0194] Fourier transform infrared spectroscopy analysis of alkaline lignin (AL) Figure 3 As shown, it is proved that the lignin synthesized by organic acid treatment has more C=O and COOH functional groups.
[0195] The peroxidase-like activity of alkaline lignin (AL) was evaluated using TMB as a substrate, and the test method was as described in Example 1. The peroxidase-like performance of the obtained material (TMB+H2O2+AL) decreased, as shown in FIG. Figure 4 As shown in a.
[0196] The catalase-like activity of alkaline lignin (AL) was evaluated using hydrogen peroxide as a substrate. The test method was as described in Example 1. The catalase-like performance of the obtained material (AL) was decreased compared with that in Example 1. Figure 4 This proves that the treatment of the present invention can effectively improve the peroxidase-like and catalase activities of lignin-based carbon dots (LCDs-OA), thereby achieving efficient adaptive ROS balancing ability.
[0197] Experimental Example 1: Test of the bactericidal performance of lignin-based carbon dots against Escherichia coli
[0198] The bactericidal performance was tested against Escherichia coli.
[0199] (1) Inoculate E. coli in LB medium and culture at 37°C and 200 rpm for 12 h in a shaking incubator. Dilute the bacterial suspension to determine the concentration of the bacterial suspension to be 10 7 CFU / mL. Take 10mL of diluted E. coli culture, add 100μL of aqueous solution (100μg / mL) of lignin carbon dots (LCDs-OA) prepared in Example 1, 100μL of 0.1mM H2O2 aqueous solution, and culture on a shaker at 37°C and 200r / min for 4h. Take 100μL of the culture solution and spread it on LB solid culture medium, culture it in a constant temperature box at 37°C for 12h, and count the colonies on the plate. The above setting is the LCDs-OA+H2O2 group.
[0200] (2) The method described in (1) above is the same except that no H2O2 aqueous solution is added. The above arrangement is the LCDs-OA group.
[0201] (3) Follow the method in (1) above, except that the sample aqueous solution is replaced with 100 μL of water. The above setting is the H2O2 group.
[0202] (4) Follow the method in (1) above, except that the sample aqueous solution is replaced with 100 μL of water and no H2O2 aqueous solution is added. The above setting is the control group (Blank).
[0203] Calculate the survival rate of E. coli and evaluate the bactericidal performance; record the number of colonies on the control plate as A0, and the number of colonies on the plate with the sample as A t , then the survival rate of E. coli is calculated as follows: Survival rate (%) = A t / A0×100%.
[0204] Fig.10 This is a plate graph showing the survival rate of Escherichia coli in the LCDs-OA+H2O2 group, LCDs-OA group, H2O2 group and control group. Fig.11 It was shown that the bactericidal rate of LCDs-OA+H2O2 against Escherichia coli was >99%, while LCDs-OA had no obvious activity in killing Escherichia coli in the absence of H2O2.
[0205] After further testing, the minimum bactericidal concentration of the lignin-based carbon dots prepared in Example 1 against Escherichia coli in the presence of H2O2 was 50 μg / mL.
[0206] Experimental Example 2: Test of the bactericidal performance of lignin-based carbon dots against Staphylococcus aureus
[0207] The test method for the bactericidal performance of the lignin-based carbon dots prepared in Example 1 against Staphylococcus aureus is as described in Experimental Example 1.
[0208] Fig.10 This is a plate graph showing the survival rate of Staphylococcus aureus in the LCDs-OA+H2O2 group, LCDs-OA group, H2O2 group and control group. Fig.11 The results show that the bactericidal rate of LCDs-OA+H2O2 against Staphylococcus aureus is >99%. However, LCDs-OA has no obvious bactericidal activity against Escherichia coli in the absence of H2O2. After further testing, the minimum bactericidal concentration of the lignin-based carbon dots prepared in Example 1 against Staphylococcus aureus in the presence of H2O2 is 50 μg / mL.
[0209] Test Example 3: Bactericidal performance test of composite materials
[0210] The bactericidal performance of the composite material prepared in Example 1 against Staphylococcus aureus or Escherichia coli was tested as described in Test Example 1(1), except that H2O2 was no longer added and the sample was replaced with 100 μL of an aqueous solution of the composite material (50, 75 or 100 μg / mL).
[0211] Fig.12 It is a plate graph of the survival rate of the composite material against Escherichia coli and Staphylococcus aureus bacterial liquid. Fig.13 It shows that the minimum bactericidal concentration of the composite material prepared in Example 1 against Staphylococcus aureus and Escherichia coli is 100 μg / mL. After replacing H2O2 in Experimental Example 1 with CaO2, the composite material still has excellent antibacterial activity in the slightly acidic environment of bacterial infection without adding H2O2.
[0212] Experimental Example 4: Cytotoxicity test of lignin-based carbon dots
[0213] The lignin-based carbon dots (LCDs-OA) in Example 1 were subjected to a cytotoxicity test on NCM-460 cells.
[0214] The cytotoxicity of LCDs-OA was investigated by MTT assay in vitro. 4 NCM-460 cells were cultured in 96-well plates at a density of 10 cells / mL overnight. Then, the cell culture medium was removed and different concentrations of LCDs-OA (0-400 μg-mL) were added to the 96-well plates. -1 ) and cultured for another 24 hours. Afterwards, the cells were gently washed twice with DPBS, and 100 μL of 0.5 mg mL -1 Fresh medium (serum-free) with MTT was added. After 4 hours of culture, the medium was discarded and 150 μL DMSO was added. The medium was gently shaken and allowed to stand for 10 minutes until the formazan formed in the cells was completely dissolved by DMSO. Then, the optical density of the cell solution was measured at a wavelength of 490 nm using a multi-mode microplate reader (Spark, Tecan).
[0215] The results are as follows Fig.14 As shown in a, the experiment found that the lignin carbon dots (LCDs-OA) in Example 1 were almost non-toxic to NCM-460 cells.
[0216] Test Example 5: Composite material cytotoxicity test
[0217] The composite material in Example 1 was subjected to a cytotoxicity test on NCM-460 cells.
[0218] The steps are the same as those described in Experimental Example 4, except that the lignin carbon dots (LCDs-OA) are replaced with a composite material.
[0219] The results are as follows Fig.14 As shown in b, the experiment found that the composite material of Example 1 had almost no toxicity to NCM-460 cells under the neutral environment of normal cells.
[0220] Test Example 6: Cellular Oxidative Damage Protection Ability Test
[0221] The ability of the lignin-based carbon dots and the composite materials in Example 1 to protect NCM-460 cells from oxidative damage was tested.
[0222] The steps were as described in Experimental Example 4, except that 50 μl of 1 mM H2O2 aqueous solution was added during the cell treatment.
[0223] The results are as follows Fig.15As shown, the experiment found that after pretreatment with the lignin carbon dots (LCDs-OA) in Example 1 and the composite material of Example 1, the cell survival rate increased in a dose-dependent manner. This shows that under the neutral environment of normal cells, both the lignin carbon dots (LCDs-OA) and the composite material have excellent cell oxidative damage protection capabilities, and the cell oxidative damage protection capability of the composite material is mainly provided by the lignin carbon dots (LCDs-OA).
[0224] Experimental Example 7: In vivo wound healing treatment experiment
[0225] Bclb / c mice (female, 7-8 weeks, purchased from Jinan Pengyue Experimental Animal Breeding Co., Ltd.) were anesthetized with 1% sodium pentobarbital 40 mg / kg. The hair on the back of the mice was removed, and an 8 mm circular wound was formed on the back of the mice. The wound was inoculated with MDR Staphylococcus aureus suspension (50 μL, 1×107 CFU / mL) and cultured for 24 hours to establish a mouse wound infection model. The mice were randomly divided into a control group and a treatment group, and were treated with a PBS buffer solution with a pH of 7.4, a solution of the composite material of Example 1 (wherein the concentration of the composite material was 1 mg / mL, and the solvent used was a PBS buffer solution with a pH of 7.4) and a solution of CaO2 (wherein the concentration of CaO2 was 1 mg / mL, and the solvent used was a PBS buffer solution with a pH of 7.4) once every 2 days. The wounds were photographed every day, and the wound area and healing rate were measured using image software. All mice were painlessly killed after 8 days of treatment, and skin wound tissues were collected, fixed with 10% paraformaldehyde, embedded in paraffin and sliced. Hematoxylin-eosin staining and Masson staining were used to observe wound healing. In addition, to verify the in vivo safety, the weight of mice was recorded every day, and the main organs (heart, liver, spleen, lung and kidney) of mice were collected for hematoxylin-eosin staining.
[0226] The results are as follows Fig.16 As shown, the experiment found that using the composite material in Example 1 to treat mouse wounds can significantly improve the wound healing speed, promote the regeneration of fibroblasts, and has no obvious physiological toxicity. Wherein I is treated with PBS buffer, II is treated with PBS solution with a concentration of 1 mg / mL composite material, and III is treated with PBS solution with a concentration of 1 mg / mL CaO2.
Claims
1. A lignin-based carbon dot composite material that is self-adaptive to wound microenvironment, characterized in that: The lignin-based carbon dot composite material is a composite material of lignin-based carbon dots and peroxides, percarbonates or persulfates.
2. The lignin-based carbon dot composite material that adapts to wound microenvironment according to claim 1, characterized in that: In the lignin-based carbon dot composite material, the mass ratio of lignin-based carbon dots to peroxide, percarbonate or persulfate is 1:1 to 1:
3.
3. The method for preparing the lignin-based carbon dot composite material capable of self-adapting to wound microenvironment according to claim 1 or 2, comprising the steps of: (1) fully dispersing lignin in deionized water; adding an organic acid and mixing uniformly; subjecting the mixture to hydrothermal treatment, filtering, dialyzing, and drying to obtain lignin-based carbon dots; (2) The lignin-based carbon dots and peroxides, percarbonates or persulfates are fully dispersed in ethanol, and the mixture is centrifuged, washed and dried to obtain a lignin-based carbon dot composite material that is adaptive to the wound microenvironment.
4. The method for preparing the lignin-based carbon dot composite material capable of self-adapting to wound microenvironment according to claim 3, characterized in that: In step (1), one or more of the following conditions are included: i. Lignin is alkaline lignin; ii. The mass ratio of lignin to deionized water is (1-3): (20-50); preferably, the mass ratio of lignin to deionized water is (1-1.5): (20-30); iii. The organic acid is oxalic acid dihydrate, citric acid or tartaric acid; preferably, the organic acid is oxalic acid dihydrate; iv. The mass ratio of lignin to the organic acid is (1-3): (1-3); preferably, the mass ratio of lignin to the organic acid is (1-2): (1-2); v. After adding the organic acid, stir at room temperature for 0.1 to 5 hours to mix evenly; preferably, stir at room temperature for 0.5 to 2 hours to mix evenly; most preferably, stir at room temperature for 1 hour to mix evenly; vi. The hydrothermal treatment temperature is 180-200°C; preferably, the hydrothermal treatment temperature is 180°C; vii. The hydrothermal treatment time is 12 to 24 hours; preferably, the hydrothermal treatment time is 12 to 15 hours; viii. The molecular weight cutoff of the dialysis bag or dialysis tube used for dialysis is 1000-3000Da, and the dialysis time is 2 to 5 days; preferably, the molecular weight cutoff of the dialysis bag or dialysis tube is 2000 to 3000Da, and the dialysis time is 2 to 3 days.
5. The method for preparing the lignin-based carbon dot composite material capable of self-adapting to wound microenvironment according to claim 3, characterized in that: In step (2), one or more of the following conditions are included: i. The peroxide is calcium peroxide, sodium peroxide, potassium peroxide or peracetic acid; the percarbonate is sodium percarbonate, potassium percarbonate or ammonium percarbonate; the persulfate is sodium permonosulfate, potassium permonosulfate, ammonium permonosulfate, potassium persulfate, sodium persulfate, ammonium persulfate, calcium persulfate, zinc persulfate or magnesium persulfate; preferably, the peroxide is calcium peroxide; ii. The mass ratio of lignin-based carbon dots to ethanol is (0.01-0.05): (20-50) g / mL; preferably, the mass ratio of lignin-based carbon dots to ethanol is (0.03-0.05): (20-30) g / mL; iii. The mass ratio of lignin-based carbon dots to peroxide, percarbonate or persulfate is (1-5): (1-5); preferably, the mass ratio of lignin-based carbon dots to peroxide, percarbonate or persulfate is (1-2): (1-2); iv. The conditions for sufficient dispersion are: stirring at room temperature for 20 to 24 hours; preferably, stirring at room temperature for 23 to 24 hours; most preferably, stirring at room temperature for 24 hours.
6. The method for preparing the lignin-based carbon dot composite material that is self-adaptive to wound microenvironment according to claim 5, characterized in that: The preparation method of calcium peroxide comprises the steps of: uniformly mixing an ammonia solution (NH3-H2O), polyethylene glycol and a CaCl2 solution, adding a hydrogen peroxide solution, and adding a NaOH solution to adjust the pH value to 10-13; and then filtering, washing and drying to obtain CaO2.
7. The method for preparing the lignin-based carbon dot composite material that is self-adaptive to wound microenvironment according to claim 6, characterized in that: Includes one or more of the following conditions: i. The concentration of the ammonia solution is 0.5 mol / L to 1 mol / L; the volume ratio of the ammonia solution to the polyethylene glycol is 1 to 5:10 to 12, preferably 1.2:12; ii. The average molecular weight of polyethylene glycol is 200 to 2000; more preferably, the average molecular weight of polyethylene glycol is 200 to 1000; most preferably, the average molecular weight of polyethylene glycol is 200 to 400; iii. The mass concentration of the hydrogen peroxide aqueous solution is 20-30%; most preferably, the mass concentration of the hydrogen peroxide aqueous solution is 25-30%; iv. The concentration of the NaOH aqueous solution is 0.1 to 0.5 mol / L; more preferably, the concentration of the NaOH aqueous solution is 0.1 to 0.2 mol / L; v. The concentration of the CaCl2 aqueous solution is 0.5-5 g / mL; the mass ratio of CaCl2 to polyethylene glycol is 3:10-12 g / mL; the volume ratio of polyethylene glycol to hydrogen peroxide aqueous solution is 10-12:1.5; vi. Aqueous hydrogen peroxide solution is added to the system in a dropwise manner; the dropwise addition rate is 1 to 5 drops per minute; preferably, the dropwise addition rate is 3 to 5 drops per minute; vii. After adding aqueous hydrogen peroxide, stir at room temperature for 1-5 hours; viii. Add NaOH aqueous solution to adjust the pH value to 11-12.
8. Application of the lignin-based carbon dot composite material adaptive to wound microenvironment as claimed in claim 1 or 2 in antibacterial; Preferably, the lignin-based carbon dot composite material is used for sterilization or inhibition of Escherichia coli or Staphylococcus aureus.
9. Use of the lignin-based carbon dot composite material that adapts to wound microenvironment as claimed in claim 1 or 2 in the production and / or removal of cellular active oxygen; Preferably, the lignin-based carbon dot composite material is used for removing or generating H2O2 in cells, or removing or generating reactive oxygen species in cells.
10. Use of the lignin-based carbon dot composite material that adapts to wound microenvironment as claimed in claim 1 or 2 in the preparation of drugs or dressings for treating bacterially infected wounds.
Citation Information
Patent Citations
Preparation method of electron beam irradiation cross-linked calcium peroxide-carbon quantum dot@ zein antibacterial membrane
CN112647193A
Solid-state luminescence pure carbon nanodot, preparation method thereof, white-light LED and visible-light communication
CN108531169A
Preparation method of lignin carbon quantum dots
CN114634815A
Cited By
Method for reducing stone cell content of pear fruits
CN121773906A