Recycling method of graphene oxide leftover material

By optimizing the stirring and dispersion and filtration of scraps in graphene oxide film production, combined with low-temperature heat treatment and vacuum hot press sintering technology, the problems of high cost and poor performance in the reuse of graphene oxide scraps are solved, and high efficiency and low cost are achieved production of graphene thermal film.

CN118954491APending Publication Date: 2024-11-15YUNNAN YUNTIAN MORION TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411071541.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing graphene oxide film scrap reuse process has problems such as high recovery cost after cutting, high energy consumption, and affecting the performance of the thermal film, and the recovered materials cannot be directly used to produce graphene films.

Method used

By adding desalinated water to the scraps after cutting edges during the production process of graphene oxide film, the solid content and viscosity are controlled, and after filtration and defoaming, coating, low-temperature heat treatment, vacuum hot press sintering and calendering processes are adopted. A graphene thermal conductive film with excellent performance was prepared.

Benefits of technology

It realizes efficient reuse of graphene oxide scraps, reduces production costs, improves the performance and yield of the thermally conductive film, and has simple process operation and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004981022130000101
    Figure BDA0004981022130000101
  • Figure HDA0004981022140000011
    Figure HDA0004981022140000011
  • Figure HDA0004981022140000012
    Figure HDA0004981022140000012
Patent Text Reader

Abstract

The invention relates to the technical field of graphene, in particular to a recycling method of graphene oxide leftover materials, which at least comprises the following steps: (1) adding desalted water into a stirring container, then adding graphene oxide film leftover materials to obtain a mixed material, and stirring and dispersing the mixed material to obtain graphene oxide slurry; (2) filtering and defoaming the graphene oxide slurry to obtain slurry to be coated; (3) coating by adopting a coating machine, and drying to obtain a graphene oxide film; and (4) sequentially carrying out low-temperature heat treatment, vacuum hot pressed sintering and calendaring on the graphene oxide film to obtain the graphene heat-conducting film. Graphene oxide film leftover materials (accounting for about 10% of the annual productivity) which are left after edge cutting in the production process of the graphene oxide film are reused, the recycled materials can be directly used for producing the graphene film, the performance of a finished film is equivalent to that of a normal heat-conducting film and even slightly higher than that of the normal heat-conducting film, the production cost is reduced, and the production efficiency is improved. And the yield is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of graphene, and in particular to a method for recycling graphene oxide scraps. Background Art

[0002] Since graphene was discovered in 2004, it has attracted attention for its ultra-high thermal conductivity (~5300W / (m·K)), and graphene thermal conductive products have been developed in recent years for heat dissipation of electronic products. With the development of graphene thermal conductive film technology, the annual production capacity of industrially prepared graphene oxide films has reached 2 million m 2 , but in the process of preparing graphene oxide film by coating and drying graphene oxide, 10wt% of cutting loss is accompanied by each production of 1 square meter of graphene oxide film, which is a great waste for raw materials and energy consumption. Reusing the cut graphene oxide film scraps has great economic value and can achieve the purpose of reducing costs and increasing efficiency. However, there are still certain problems in the existing reuse process of graphene oxide film scraps. For example, Chinese patent (publication number is CN 117735539A) discloses a method for manufacturing graphene oxide and recycling scraps, by adjusting the pH value of graphene oxide coating scraps and boiling at high temperature, then adding graphene oxide slurry to obtain a recycled finished product, but it is necessary to add a pH regulator, and it is also necessary to add graphene oxide slurry, and the recycled material cannot be directly used for the production of graphene film, which increases the recovery cost and recovery process, and it is necessary to realize recovery at high temperature, which increases energy consumption, which is not conducive to realizing large-scale industrial promotion. Summary of the invention

[0003] In order to solve the above problems, the present invention provides a method for recycling graphene oxide scraps, which reuses the graphene oxide film scraps (accounting for about 10% of the annual production capacity) left over from the trimming process of the graphene oxide film production and is about to be discarded. The recycled materials can be directly used to produce graphene films, and the performance of the finished film is equivalent to that of a normal thermal conductive film, or even slightly higher than that of a normal thermal conductive film, thereby reducing production costs and improving yields.

[0004] The present invention provides a method for recycling graphene oxide scraps, which comprises at least the following steps:

[0005] (1) adding desalted water into a stirring container, then adding graphene oxide film scraps to obtain a mixed material, and stirring and dispersing the mixed material to obtain graphene oxide slurry;

[0006] (2) filtering and defoaming the graphene oxide slurry to obtain a slurry to be coated;

[0007] (3) coating with a coating machine and drying to obtain a graphene oxide film;

[0008] (4) The graphene oxide film is subjected to low-temperature heat treatment, vacuum hot pressing sintering, and rolling in sequence to obtain a graphene thermal conductive film.

[0009] The graphene oxide film scraps described in the present invention are obtained by scraping, drying, peeling and cutting the graphene oxide slurry prepared by the Hummers method.

[0010] As a preferred technical solution, the specifications of the graphene oxide scraps are: length ≤ 1m, width ≤ 15cm. Preferably, the specifications of the graphene oxide scraps are: length ≤ 20m, width ≤ 10cm.

[0011] As a preferred technical solution, step (1) is: adding desalted water into a stirring container, then adding graphene oxide film scraps for soaking, then adding desalted water to obtain a mixed material, and stirring and dispersing the mixed material to obtain graphene oxide slurry.

[0012] As a preferred technical solution, the soaking time is ≥12h, preferably 24h.

[0013] As a preferred technical solution, the mass proportion of graphene oxide film scraps in the mixed material is 6-7%, preferably 6.2-6.5%.

[0014] As a preferred technical solution, the solid content of the graphene oxide slurry is 3-6wt%, and the viscosity is 5000-15000cps at 25°C. Preferably, the solid content of the graphene oxide slurry is 4-5wt%, and the viscosity is 8000-13000cps at 25°C.

[0015] As a preferred technical solution, when the graphene oxide film scraps are not soaked in desalted water, the stirring and dispersion is specifically as follows: the stirring and dispersion time is ≥4h, the speed of the high-speed stirring paddle in the first hour is 200-300r / min, and the speed of the low-speed stirring paddle in the first hour is 10-15r / min; the speed of the high-speed stirring paddle after the first hour is 500-700r / min, and the speed of the low-speed stirring paddle after the first hour is 10-15r / min.

[0016] As a preferred technical solution, when the graphene oxide film scraps are soaked in desalted water, the stirring and dispersion is specifically as follows: the stirring and dispersion time is ≥2h, the speed of the high-speed stirring paddle is 1500-2500r / min, and the speed of the low-speed stirring paddle is 20-80r / min.

[0017] The purpose of the present invention is to make full use of the graphene oxide film scraps left over from the cutting process of the graphene oxide film production process. However, when the graphene oxide film scraps are recycled, there are convex points on the surface of the coating film, which affects the performance of the subsequent graphene thermal conductive film. The present invention optimizes the reuse process and recycles the graphene oxide film scraps without increasing the recycling cost to obtain a graphene oxide film product with excellent comprehensive performance. Specifically, the present invention controls the amount of desalted water added to the mixed material, and optimizes the stirring and dispersing process to obtain a graphene oxide slurry with a solid content of 3-6wt% and a viscosity of 5000-15000cps at 25°C, so that the scraps undergo a reversible reaction and are fully dispersed into a graphene oxide slurry, which is easy to carry out a subsequent filtration process, ensuring the subsequent coating uniformity and coating flatness, thereby ensuring the final performance of the product. Without the above stirring and dispersing process, if the amount of desalted water added is too low or the viscosity of the graphite oxide slurry is too high, the dispersibility of the graphene oxide film scraps will be adversely affected, increasing the difficulty of subsequent filtration, affecting the coating uniformity and film flatness, and thus affecting the final performance of the product. In addition, the thermal conductivity of the product obtained by the subsequent filtration and defoaming treatment of the graphene oxide slurry obtained by homogenizing the graphene oxide slurry in the early stage of the present invention is low, so the present invention does not perform homogenization.

[0018] Furthermore, the graphene oxide film scraps obtained during the production process of the graphene oxide film are generally of relatively long specifications and need to be further cut and then mixed with desalted water to improve the dispersibility of the scraps in the desalted water and reduce damage to the equipment. In addition, the cutting process needs to avoid excessive local temperature that may lead to reduction of the graphene oxide and thus affect its dispersion performance.

[0019] As a preferred technical solution, the filtering specifically comprises: passing the graphene oxide slurry through a filter with a pore size of 300-800 μm and a filter with a pore size of ≤200 μm in sequence.

[0020] Preferably, the filtering specifically comprises: passing the graphene oxide slurry through a filter with a pore size of 500 μm and a filter with a pore size of 100 μm in sequence.

[0021] As a preferred technical solution, the number of filters with a pore size of 300-800 μm is 1-5, preferably 2-3.

[0022] As a preferred technical solution, the number of filters with a pore size of ≤200 μm is 2-5, preferably 3-4.

[0023] Preferably, the graphene oxide slurry is cooled after passing through the first filter with a pore size of 100 μm, and defoamed before passing through the last filter with a pore size of 100 μm.

[0024] Preferably, the filtering is specifically as follows: the graphene oxide slurry is sequentially passed through filters 1 and 2 with a pore size of 500 μm, a filter 1 with a pore size of 100 μm, and after cooling, passed through a filter 2 with a pore size of 100 μm, and after defoaming, passed through a filter 3 with a pore size of 100 μm to obtain the slurry to be coated.

[0025] The inventors discovered during the course of their research that by filtering and defoaming the graphene oxide slurry before coating, especially by passing the graphene oxide slurry through 2-3 filters with a pore size of 500 μm and 3-4 filters with a pore size of 100 μm in sequence, and controlling the graphene oxide slurry to be cooled after passing through the first filter with a pore size of 100 μm, and defoaming before passing through the last filter with a pore size of 100 μm, the subsequent coating uniformity and coating film flatness can be ensured, the generation of film bumps can be effectively avoided, and the normal progress of subsequent processes and the comprehensive performance of subsequent products can be ensured.

[0026] As a preferred technical solution, the coater is a wire blade coater, and the thickness of the graphene oxide film is 100 μm-300 μm, preferably 200-300 μm.

[0027] As a preferred technical solution, the low-temperature heat treatment is specifically as follows: stacking the graphene oxide film according to the final target thickness of the finished graphene film, separating each stack with natural graphite paper, placing the dry-stacked multi-layer graphene oxide film into a graphite crucible / jig / clamp together, and the total height of the graphene oxide film does not exceed 100 cm. The crucible / jig / clamp containing the graphene oxide film is placed in an oven, and heated from 20-30°C to 150-180°C at a rate of 0.3-1°C / min to obtain a low-temperature heat-treated film.

[0028] As a preferred technical solution, the vacuum hot pressing sintering is specifically as follows: the low temperature heat treated film is moved into a vacuum hot pressing sintering furnace, and the vacuum degree is first drawn to 5×10 -2 -1×10 -4 Pa, and then heated to 2600-2700°C at a rate of 5-50°C / min, and then applied 20-150MPa pressure on the graphene film product and maintained during the heating process, and maintained at the highest temperature for 2-4h to obtain a vacuum hot-pressed sintered film.

[0029] As a preferred technical solution, the calendering is specifically as follows: the natural graphite paper in the vacuum hot pressing sintered film is removed and placed in a vacuum hydraulic press, and the air pressure in the calendering chamber is first pumped to 1×10 -3 Pa, and then apply a pressure of 50-180MPa for 5-10min to obtain a graphene thermal conductive film.

[0030] As a preferred technical solution, the planar thermal conductivity of the graphene thermally conductive film is 1100-1400 W / (m·K).

[0031] As a preferred technical solution, the density of the graphene thermal conductive film is 2.00-2.15g / cm 3 , preferably 2.05-2.12 g / cm 3 .

[0032] The present invention prepares a graphene thermal conductive film with a planar thermal conductivity of 1100-1400 W / (m·K) by sequentially subjecting a graphene oxide film to low-temperature heat treatment, vacuum hot pressing sintering, and calendering. The scraps that should be counted as production loss are re-prepared into a graphene oxide film, effectively improving the yield by about 7% and reducing the production cost.

[0033] The recycling process provided by the present invention only needs to use desalted water, and each process flow is designed for batch production, which is convenient and fast to operate and improves production efficiency.

[0034] Beneficial Effects

[0035] 1. The present invention provides a method for recycling graphene oxide scraps, which reuses the graphene oxide film scraps (accounting for about 10% of the annual production capacity) left over from the cutting process of the graphene oxide film production and are about to be discarded. The recycled materials can be directly used to produce graphene films, and the performance of the finished film is equivalent to that of a normal thermal conductive film, or even slightly higher than that of a normal thermal conductive film, thereby reducing production costs and improving yields.

[0036] 2. The present invention controls the amount of desalted water added to the mixture and optimizes the stirring and dispersing process to obtain a graphite oxide slurry with a solid content of 3-6wt% and a viscosity of 5000-15000cps at 25°C, so that the scraps undergo a reversible reaction and are fully dispersed into graphene oxide slurry, which is easy to carry out a subsequent filtration process, thereby ensuring the subsequent coating uniformity and coating film flatness, thereby ensuring the final performance of the product.

[0037] 3. The present invention filters and defoams the graphene oxide slurry before coating, especially passes the graphene oxide slurry through 2-3 filters with a pore size of 500 μm and 3-4 filters with a pore size of 100 μm in sequence, and controls the graphene oxide slurry to be cooled after passing through the first filter with a pore size of 100 μm, and defoams before passing through the last filter with a pore size of 100 μm, so as to ensure the uniformity of subsequent coating and the flatness of the coating film, effectively avoid the generation of film bumps, and ensure the normal progress of subsequent processes and the comprehensive performance of subsequent products.

[0038] 4. The present invention prepares a graphene thermal conductive film with a planar thermal conductivity of 1100-1400 W / (m·K) by sequentially subjecting the graphene oxide film to low-temperature heat treatment, vacuum hot pressing sintering, and calendering. The scraps that should have been counted as production loss are re-prepared into a graphene oxide film, which effectively improves the yield by about 7% and reduces the production cost.

[0039] 5. The recycling process provided by the present invention only needs to use desalted water, and the scraps of graphene oxide film can be recycled to obtain graphene oxide film products with excellent comprehensive performance without increasing the recycling cost. All process flows are designed for batch production, which is convenient and fast to operate and improves production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a diagram of the graphene thermal conductive film product provided in Example 1 of the present invention.

[0041] Figure 2 This is a picture of the graphene thermal conductive film product provided for Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0042] Example 1

[0043] Embodiment 1 of the present invention provides a method for recycling graphene oxide scraps, comprising the following steps:

[0044] (1) adding 1407 kg of desalted water into a stirring container, and then adding 93 kg of graphene oxide film scraps to obtain a mixed material, and stirring and dispersing the mixed material to obtain a graphene oxide slurry;

[0045] (2) filtering and defoaming the graphene oxide slurry to obtain a slurry to be coated;

[0046] (3) coating with a coating machine and drying to obtain a graphene oxide film;

[0047] (4) The graphene oxide film is subjected to low-temperature heat treatment, vacuum hot pressing sintering, and rolling in sequence to obtain a graphene thermal conductive film.

[0048] The graphene oxide film scraps described in this embodiment are obtained by scraping, drying, peeling and cutting the graphene oxide slurry prepared by the Hummers method.

[0049] The specifications of the graphene oxide scraps are: length ≤ 20m, width ≤ 10cm.

[0050] The weight proportion of graphene oxide film scraps in the mixed material is 6.2%.

[0051] The stirring and dispersing is specifically as follows: the stirring and dispersing time is 4 hours, the speed of the high-speed stirring paddle in the first hour is 250 r / min, and the speed of the low-speed stirring paddle in the first hour is 10 r / min; the speed of the high-speed stirring paddle after the first hour is 600 r / min, and the speed of the low-speed stirring paddle after the first hour is 15 r / min.

[0052] The graphene oxide slurry has a solid content of 4.5 wt % and a viscosity of 10000 cps at 25° C.

[0053] The filtering is specifically as follows: the graphene oxide slurry is sequentially passed through filters 1 and 2 with a pore size of 500 μm, a filter 1 with a pore size of 100 μm, and after cooling, passed through a filter 2 with a pore size of 100 μm, and after defoaming, passed through a filter 3 with a pore size of 100 μm to obtain the slurry to be coated.

[0054] The coating machine is a wire blade coating machine, and the thickness of the graphene oxide film is 200 μm (3000 sheets of 350 mm*350 mm*200 μm graphene oxide films).

[0055] The low-temperature heat treatment is specifically as follows: stacking the graphene oxide film according to the final target thickness of the finished graphene film, separating each stack with natural graphite paper, placing the dry-stacked multi-layer graphene oxide film into a graphite crucible / jig / clamp together, with the total height of the graphene oxide film not exceeding 100 cm, placing the crucible / jig / clamp containing the graphene oxide film into an oven, and heating from 25°C to 160°C at a rate of 0.5°C / min to obtain a low-temperature heat-treated film.

[0056] The vacuum hot pressing sintering is specifically as follows: the low temperature heat treated film is moved into a vacuum hot pressing sintering furnace, and the vacuum degree is first drawn to 5×10 -2 Pa, and then heated to 2600°C at a rate of 25°C / min, and then applied and maintained a pressure of 100MPa on the graphene film product during the heating process, and maintained at the highest temperature for 3h to obtain a vacuum hot-pressed sintered film.

[0057] The calendering process is as follows: the natural graphite paper in the vacuum hot pressing sintered film is removed and placed in a vacuum hydraulic press, and the air pressure in the calendering chamber is first pumped down to 1×10 -3 Pa, and then apply a pressure of 100MPa for 8min to obtain a graphene thermal conductive film (333mm*329mm*371μm).

[0058] The planar thermal conductivity of the graphene thermal conductive film is 1350 W / (m·K).

[0059] The density of the graphene thermal conductive film is 2.05 g / cm 3 .

[0060] Example 2

[0061] Embodiment 2 of the present invention provides a method for recycling graphene oxide scraps, comprising the following steps:

[0062] (1) adding 300 kg of desalted water into a stirring container, then adding 36 kg of graphene oxide film scraps for soaking, and then adding 217 kg of desalted water to obtain a mixed material, and stirring and dispersing the mixed material to obtain a graphene oxide slurry;

[0063] (2) filtering and defoaming the graphene oxide slurry to obtain a slurry to be coated;

[0064] (3) coating with a coating machine and drying to obtain a graphene oxide film;

[0065] (4) The graphene oxide film is subjected to low-temperature heat treatment, vacuum hot pressing sintering, and rolling in sequence to obtain a graphene thermal conductive film.

[0066] The graphene oxide film scraps described in this embodiment are obtained by scraping, drying, peeling and cutting the graphene oxide slurry prepared by the Hummers method.

[0067] The specifications of the graphene oxide scraps are: length ≤ 20m, width ≤ 10cm.

[0068] The soaking time is 24 hours.

[0069] The weight proportion of graphene oxide film scraps in the mixed material is 6.5%.

[0070] The stirring and dispersing process is as follows: the stirring and dispersing time is 2 hours, the rotation speed of the high-speed stirring paddle is 1750 r / min, and the rotation speed of the low-speed stirring paddle is 40 r / min.

[0071] The graphene oxide slurry has a solid content of 4.5 wt % and a viscosity of 10000 cps at 25° C.

[0072] The filtering is specifically as follows: the graphene oxide slurry is sequentially passed through filters 1 and 2 with a pore size of 500 μm, a filter 1 with a pore size of 100 μm, and after cooling, passed through a filter 2 with a pore size of 100 μm, and after defoaming, passed through a filter 3 with a pore size of 100 μm to obtain the slurry to be coated.

[0073] The coating machine is a wire blade coating machine, and the thickness of the graphene oxide film is 300 μm (1000 sheets of 57 mm*339 mm*300 μm graphene oxide films).

[0074] The low-temperature heat treatment is specifically as follows: stacking the graphene oxide film according to the final target thickness of the finished graphene film, separating each stack with natural graphite paper, placing the dry-stacked multi-layer graphene oxide film into a graphite crucible / jig / clamp together, with the total height of the graphene oxide film not exceeding 100 cm, placing the crucible / jig / clamp containing the graphene oxide film into an oven, and heating from 25°C to 160°C at a rate of 0.5°C / min to obtain a low-temperature heat-treated film.

[0075] The vacuum hot pressing sintering is specifically as follows: the low temperature heat treated film is moved into a vacuum hot pressing sintering furnace, and the vacuum degree is first drawn to 5×10 -2 Pa, and then heated to 2600°C at a rate of 25°C / min, and then applied and maintained a pressure of 100MPa on the graphene film product during the heating process, and maintained at the highest temperature for 3h to obtain a vacuum hot-pressed sintered film.

[0076] The calendering process is as follows: the natural graphite paper in the vacuum hot pressing sintered film is removed and placed in a vacuum hydraulic press, and the air pressure in the calendering chamber is first pumped down to 1×10 -3 Pa, and then apply a pressure of 100MPa for 8min to obtain a graphene thermal conductive film (333mm*329mm*371μm).

[0077] The planar thermal conductivity of the graphene thermal conductive film is 1379.3 W / (m·K).

[0078] The density of the graphene thermal conductive film is 2.12 g / cm 3 .

[0079] Example 3

[0080] Embodiment 3 of the present invention provides a method for recycling graphene oxide scraps, comprising the following steps:

[0081] (1) adding 1410 kg of desalted water into a stirring container, then adding 90 kg of graphene oxide film scraps to obtain a mixed material, and stirring and dispersing the mixed material to obtain a graphene oxide slurry;

[0082] (2) filtering and defoaming the graphene oxide slurry to obtain a slurry to be coated;

[0083] (3) coating with a coating machine and drying to obtain a graphene oxide film;

[0084] (4) The graphene oxide film is subjected to low-temperature heat treatment, vacuum hot pressing sintering, and rolling in sequence to obtain a graphene thermal conductive film.

[0085] The graphene oxide film scraps described in this embodiment are obtained by scraping, drying, peeling and cutting the graphene oxide slurry prepared by the Hummers method.

[0086] The specifications of the graphene oxide scraps are: length ≤ 20m, width ≤ 10cm.

[0087] The weight proportion of graphene oxide film scraps in the mixed material is 6%.

[0088] The stirring and dispersing is specifically as follows: the stirring and dispersing time is 4 hours, the speed of the high-speed stirring paddle in the first hour is 250 r / min, and the speed of the low-speed stirring paddle in the first hour is 10 r / min; the speed of the high-speed stirring paddle after the first hour is 600 r / min, and the speed of the low-speed stirring paddle after the first hour is 15 r / min.

[0089] The graphene oxide slurry has a solid content of 3.9 wt % and a viscosity of 8900 cps at 25° C.

[0090] The filtering is specifically as follows: the graphene oxide slurry is sequentially passed through filters 1 and 2 with a pore size of 500 μm, a filter 1 with a pore size of 100 μm, and after cooling, passed through a filter 2 with a pore size of 100 μm, and after defoaming, passed through a filter 3 with a pore size of 100 μm to obtain the slurry to be coated.

[0091] The coating machine is a wire blade coating machine, and the thickness of the graphene oxide film is 200 μm (3000 sheets of 350 mm*350 mm*200 μm graphene oxide films).

[0092] The low-temperature heat treatment is specifically as follows: stacking the graphene oxide film according to the final target thickness of the finished graphene film, separating each stack with natural graphite paper, placing the dry-stacked multi-layer graphene oxide film into a graphite crucible / jig / clamp together, with the total height of the graphene oxide film not exceeding 100 cm, placing the crucible / jig / clamp containing the graphene oxide film into an oven, and heating from 25°C to 160°C at a rate of 0.5°C / min to obtain a low-temperature heat-treated film.

[0093] The vacuum hot pressing sintering is specifically as follows: the low temperature heat treated film is moved into a vacuum hot pressing sintering furnace, and the vacuum degree is first drawn to 5×10 -2 Pa, and then heated to 2600°C at a rate of 25°C / min, and then applied and maintained a pressure of 100MPa on the graphene film product during the heating process, and maintained at the highest temperature for 3h to obtain a vacuum hot-pressed sintered film.

[0094] The calendering process is as follows: the natural graphite paper in the vacuum hot pressing sintered film is removed and placed in a vacuum hydraulic press, and the air pressure in the calendering chamber is first pumped down to 1×10-3 Pa, and then apply a pressure of 100MPa for 8min to obtain a graphene thermal conductive film (333mm*329mm*371μm).

[0095] The planar thermal conductivity of the graphene thermal conductive film is 1230 W / (m·K).

[0096] The density of the graphene thermal conductive film is 2.08 g / cm 3 .

[0097] Example 4

[0098] Compared with Example 1, the difference of this embodiment is that the amount of graphene oxide film scraps added is 105kg. The mass proportion of graphene oxide film scraps in the mixed material is 6.9%. The solid content of the graphene oxide slurry is 5.2wt%, and the viscosity is 12000cps at 25°C. The density of the graphene thermal conductive film is 2.11g / cm 3 The planar thermal conductivity of the graphene thermal conductive film is 1280 W / (m·K).

[0099] Comparative Example 1

[0100] Compared with Example 1, the difference of this embodiment is that the amount of graphene oxide film scraps added is 120kg. The mass proportion of graphene oxide film scraps in the mixed material is 7.9%. The solid content of the graphene oxide slurry is 5.9wt%, and the viscosity is 12700cps at 25°C. The density of the graphene thermal conductive film is 2.04g / cm 3 The in-plane thermal conductivity of the graphene thermal conductive film is 1136 W / (m·K).

[0101] Comparative Example 2

[0102] Compared with Example 1, the difference of this embodiment is that the amount of graphene oxide film scraps added is 80kg. The mass proportion of graphene oxide film scraps in the mixed material is 5.4%. The solid content of the graphene oxide slurry is 4.4wt%, and the viscosity is 9600cps at 25°C. The density of the graphene thermal conductive film is 2.05g / cm 3 The in-plane thermal conductivity of the graphene thermal conductive film is 1169 W / (m·K).

[0103] Comparative Example 3

[0104] Compared with Example 1, the difference of this embodiment is that, during the preparation process, step (2) does not filter the graphene oxide slurry. The amount of graphene oxide film scraps added is 90kg, and the mass proportion of graphene oxide film scraps in the mixed material is 6%. The solid content of the graphene oxide slurry is 4.5wt%, and the viscosity is 10000cps at 25°C. The density of the graphene thermal conductive film is 2.11g / cm 3 The in-plane thermal conductivity of the graphene thermal conductive film is 1244 W / (m·K).

[0105] Performance Testing

[0106] According to the standard GB / T 22588-2008 "Flash Method for Measurement of Thermal Diffusivity or Thermal Conductivity", the graphene thermal conductive films obtained in Examples 1-4 and Comparative Examples 1-3 were tested for in-plane thermal conductivity. The samples were cut into 13*4.5 mm long and thin strips, stacked into blocks with a thickness of about 10 mm, placed in a test stand, and fixed before adjusting the test parameters. Before measuring the in-plane thermal conductivity, the surface of the graphene thermal conductive film was observed to see if there was any poor appearance. The test data of appearance inspection and in-plane thermal conductivity are recorded in Table 1.

[0107] Table 1

[0108]

Claims

1. A method for recycling graphene oxide scraps, characterized in that: At least the following steps are included: (1) adding desalted water into a stirring container, then adding graphene oxide film scraps to obtain a mixed material, and stirring and dispersing the mixed material to obtain graphene oxide slurry; (2) filtering and defoaming the graphene oxide slurry to obtain a slurry to be coated; (3) coating with a coating machine and drying to obtain a graphene oxide film; (4) The graphene oxide film is subjected to low-temperature heat treatment, vacuum hot pressing sintering, and rolling in sequence to obtain a graphene thermal conductive film.

2. The method for recycling graphene oxide scraps according to claim 1, characterized in that: The step (1) is: adding desalted water into a stirring container, then adding graphene oxide film scraps for soaking, then adding desalted water to obtain a mixed material, and stirring and dispersing the mixed material to obtain graphene oxide slurry.

3. The method for recycling graphene oxide scraps according to claim 1 or 2, characterized in that: The weight proportion of graphene oxide film scraps in the mixed material is 6-7%.

4. The method for recycling graphene oxide scraps according to claim 3, characterized in that: The graphene oxide slurry has a solid content of 3-6wt% and a viscosity of 5000-15000cps at 25°C.

5. The method for recycling graphene oxide scraps according to claim 4, characterized in that: The filtering specifically comprises: passing the graphene oxide slurry through a filter with a pore size of 300-800 μm and a filter with a pore size of ≤200 μm in sequence.

6. The method for recycling graphene oxide scraps according to claim 5, characterized in that: The number of the filters with a pore size of 300-800 μm is 1-5, preferably 2-3.

7. The method for recycling graphene oxide scraps according to claim 5, characterized in that: The number of the filters with a pore size of ≤200 μm is 2-5, preferably 3-4.

8. The method for recycling graphene oxide scraps according to claim 1, characterized in that: The low-temperature heat treatment is specifically as follows: stacking the graphene oxide film according to the final target thickness of the finished graphene film, separating each stack with natural graphite paper, placing the dry-stacked multi-layer graphene oxide film into a graphite crucible / jig / clamp together, with the total height of the graphene oxide film not exceeding 100 cm, placing the crucible / jig / clamp containing the graphene oxide film into an oven, and heating from 20-30°C to 150-180°C at a rate of 0.3-1°C / min to obtain a low-temperature heat-treated film.

9. The method for recycling graphene oxide scraps according to claim 8, characterized in that: The vacuum hot pressing sintering is specifically as follows: the low temperature heat treated film is moved into a vacuum hot pressing sintering furnace, and the vacuum degree is first drawn to 5×10 -2 -1×10 -4 Pa, and then heated to 2600-2700°C at a rate of 5-50°C / min, and then applied 20-150MPa pressure on the graphene film product and maintained during the heating process, and maintained at the highest temperature for 2-4h to obtain a vacuum hot-pressed sintered film.

10. The method for recycling graphene oxide scraps according to claim 9, characterized in that: The calendering process is as follows: the natural graphite paper in the vacuum hot pressing sintered film is removed and placed in a vacuum hydraulic press, and the air pressure in the calendering chamber is first pumped down to 1×10 -3 Pa, and then apply a pressure of 50-180MPa for 5-10min to obtain a graphene thermal conductive film.