Preparation method and application of ultrathin MoS2 nanosheet
Through hydrothermal synthesis and surfactant-assisted ball milling technology, combined with ice-water bath ultrasonic and freeze-drying, the thickness unevenness and stacking of ultra-thin MoS2 nanosheets were solved, and nanosheets with high stability and suitable for industrial production were prepared. It exhibits excellent friction performance in the field of lubrication.
Patent Information
- Application Number
- CN202410986848.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, when preparing ultra-thin MoS2 nanosheets, there are problems of layer thickness unevenness and large-area stacking, which is difficult to meet the needs of industrial production and high-performance applications.
The hydrothermal synthesis method is used to react the metal molybdenum salt and sulfur salt in a mixed solution of polyethylene glycol and deionized water, combined with surfactant-assisted high-speed ball milling and ice water bath ultrasonic technology, through fine centrifugation and freeze-drying steps, Ultrathin MoS2 nanosheets without large area stacking were prepared.
The thickness of MoS2 nanosheets is controlled and uniformly dispersed, with stable particle size, and exhibits low coefficient of friction and slight wear in lubricating applications, meeting the needs of industrial production and high-performance applications.
Smart Images

Figure CN118954597A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nanomaterials, and in particular to a method for preparing an ultra-thin MoS2 nanosheet and applications thereof. Background Art
[0002] Transition metal disulfide MoS2 is a typical two-dimensional layered material, with weak van der Waals forces between layers. If the van der Waals force is destroyed by an external force, the bulk molybdenum disulfide will be peeled off into a few nanosheets. The molybdenum disulfide nanosheets obtained after peeling are widely used in hot fields such as optoelectronic devices, lubricating materials, and catalysis. At present, the molybdenum disulfide powder sold on the market is a natural or synthetic bulk material. The molybdenum disulfide has low purity, large blocks, and a particle size of large micrometers. Therefore, it is of great significance to develop a simple and easy preparation method with good yield and quality.
[0003] Traditional MoS2 preparation methods, such as chemical vapor deposition (CVD) and mechanical exfoliation, can produce high-quality samples, but they have limitations in large-scale production and layer thickness uniformity. Especially in the pursuit of large-scale preparation of ultra-thin MoS2 nanosheets, in materials science, when referring to "ultra-thin molybdenum disulfide (MoS2) nanosheets", "ultra-thin" usually refers to the thickness of these nanosheets at the atomic level or the order of a few atomic layers. However, MoS2 prepared by the above method has uneven nanosheet stacking, resulting in poor uniformity of MoS2 nanosheet thickness. How to efficiently and economically achieve controllable thickness and uniform dispersion has become a technical problem that needs to be solved urgently.
[0004] The present invention aims to overcome the deficiencies in the prior art and provide a method for preparing ultrathin MoS2 nanosheets which is easy to operate, highly repeatable and has no large-area stacking of MoS2 nanosheets, thereby meeting the needs of industrial production and high-performance applications. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing ultrathin MoS2 nanosheets and application thereof, so as to improve the problems existing in the prior art.
[0006] On the one hand, the present invention provides a method for preparing ultrathin MoS2 nanosheets, which specifically comprises:
[0007] S1, adding metal molybdenum salt and sulfur salt to a mixed solution of polyethylene glycol and deionized water, mixing evenly, sealing and using a hydrothermal synthesis method to obtain nano MoS2;
[0008] S2, dispersing nano-MoS2 in a surfactant solvent, and processing by high-speed ball milling to obtain a uniform MoS2 nanosheet suspension;
[0009] S3, centrifuging the MoS2 nanosheet suspension at 4000 rpm, collecting 1 / 2 of the upper suspension and performing continuous ice-water bath sonication, centrifuging the mixed solution after ice-water bath sonication at a low speed for the first time, collecting 1 / 2 of the upper filtrate and performing a second ice-water bath sonication, and collecting 1 / 2 of the upper filtrate by a second high-speed centrifugation to obtain an ultrathin MoS2 nanosheet solution;
[0010] S4. Freeze the ultrathin MoS2 nanosheet solution in a refrigerator at below -25°C for 20-25 hours, and freeze-dry it in a freeze dryer at -70 to -80°C for three to four days to obtain ultrathin MoS2 nanosheets.
[0011] More preferably, in step S1, the metal molybdenum salt is one of sodium molybdate, ammonium molybdate, and ammonium molybdate tetrahydrate; the sulfur salt is one of thiourea, L-cysteine, and thioacetamide; the molar ratio of the metal molybdenum salt to the sulfur salt is 1:(4-10); the molecular weight of the polyethylene glycol is 200-800, wherein the mass fraction ratio of the polyethylene glycol to deionized water is (20wt%-60wt%):(40wt%-80wt%); the temperature in the hydrothermal synthesis method is 180-220°C, and the reaction time is 18-24h.
[0012] More preferably, in step S2, the surfactant is one or two of saponin, N-methylpyrrolidone, isopropanol, and N-dimethylformamide.
[0013] More preferably, in step S2, the mass ratio of nano-MoS2, deionized water and surfactant is (1-7):12:(1-7).
[0014] More preferably, in step S2, the grinding balls used in the high-speed ball milling are 3 mm zirconia balls, the ball-to-material mass ratio is (5-20):1, the rotation speed is 400-600 rpm, and the ball milling time is 8-20 h.
[0015] More preferably, in step S3, ice bath ultrasonic treatment is performed, the ice pack and water are replaced every 30 minutes to maintain the water temperature at 25°C, the time is 8-12 hours, and the ultrasonic power is 220-300W.
[0016] More preferably, in step S3, the first centrifugation speed is 3500-5000 rpm, and the time is 8-10 min; the second centrifugation speed is 10000-12000 rpm, and the time is 15-30 min.
[0017] In the second aspect, the present invention provides an application of ultrathin MoS2 nanosheets, using ultrathin MoS2 nanosheets prepared by any of the above preparation methods, and using MoS2 nanosheets as acid liquid lubricating additives or ultrathin MoS2 nanosheets as alcohol liquid lubricating additives; wherein the acid liquid includes boric acid solution, citric acid solution, and oxalic acid solution; the alcohol liquid includes glycerol solution, 1-3 propylene glycol solution, and 1-4 butanediol solution.
[0018] More preferably, MoS2 is used at a concentration of 1.0 wt%.
[0019] More preferably, when ultra-thin MoS2 nanosheets are used as acid liquid lubricant additives, the friction pair is silicon nitride balls and silicon-doped diamond film disks; when ultra-thin MoS2 nanosheets are used as alcohol liquid lubricant additives, the friction pair is silicon nitride balls and sapphire disks.
[0020] Compared with the prior art, the advantages of the present invention are:
[0021] First, hydrothermal synthesis, as a mild and effective chemical synthesis method, can achieve material assembly and structural control at the molecular level by precisely controlling reaction conditions. Surfactant-assisted ball milling technology is an efficient nanomaterial dispersion and size control method developed in recent years. Through the action of mechanical force, nanoscale refinement and uniform dispersion can be achieved while maintaining the structural integrity of nanomaterials, especially in the preparation of ultra-thin MoS2. In this context, combining hydrothermal synthesis with surfactant-assisted ball milling technology, supplemented by fine centrifugal separation and washing steps, and subsequent freeze-drying treatment, a novel preparation method can be developed that can not only ensure the ultra-thin characteristics of MoS2 nanosheets, but also achieve efficient separation and purification. This method is simple to operate, highly reproducible, and the prepared MoS2 nanosheets do not have large-area stacking.
[0022] Secondly, the inventors have found through research that from the scanning electron microscope images of MoS2 nanosheets, it can be found that their particle size is stable at 100-500nm, and the morphology of the MoS2 nanosheets prepared by this preparation method is stable, without large-area stacking; subsequently, the ultra-thin MoS2 nanosheets are dispersed in a water-based lubricating fluid in the form of ultrasonic dispersion, and the lubrication performance is tested with silicon nitride Si3N4 balls and silicon-doped diamond-like film disks and silicon nitride Si3N4 balls and sapphire disks as friction pairs, which can obtain ultra-low friction coefficients and slight wear. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a SEM picture of molybdenum disulfide after hydrothermal synthesis in Example 1 of the present invention;
[0024] Figure 2This is a SEM picture of molybdenum disulfide after high-speed ball milling in Example 1 of the present invention;
[0025] Figure 3 This is a SEM picture of molybdenum disulfide after low-temperature cooling and freeze-drying in Example 1 of the present invention;
[0026] Figure 4 This is a SEM picture of molybdenum disulfide after high-speed ball milling in Example 2 of the present invention;
[0027] Figure 5 This is a SEM picture of molybdenum disulfide after low-temperature cooling and freeze-drying in Example 2 of the present invention;
[0028] Figure 6 This is the friction curve of molybdenum disulfide as a nano-lubricating additive in a boric acid solution system;
[0029] Figure 7 This is a SEM image of the wear scar on the surface of a silicon-doped diamond-like film disk lubricated with a boric acid solution containing ultra-thin MoS2 nanosheets;
[0030] Figure 8 This is the friction curve of molybdenum disulfide as a nano-lubricating additive in a propylene glycol solution system;
[0031] Fig. 9 This is a SEM image of the wear marks on the sapphire disk surface lubricated with propylene glycol solution with ultra-thin MoS2 nanosheets. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.
[0033] Embodiment 1:
[0034] A method for preparing MoS2 nanosheets, the specific steps are as follows:
[0035] (1) Weigh 2 mmol of sodium molybdate and 8 mmol of L-cysteine and dissolve them in 30 mL of deionized water and 30 mL of polyethylene glycol 200 to form a reaction solution. After stirring and ultrasonicating for 1.5 min each, transfer the mixture to a 100 mL reactor and react at 200° C. for 20 h. After the reaction is completed, naturally cool the mixture to room temperature. Filter the reaction product to obtain a black precipitate, wash it with deionized water and ethanol several times, and dry it in a vacuum drying oven at 70° C. for 8 h.
[0036] (2) The MoS2 powder synthesized in step (1) is mixed with deionized water and saponin in a mass ratio of 1:6:3 to obtain 50 g of a mixed solution, and the mixed solution is subjected to ultrasonic treatment and stirring at room temperature (25°C) at a power of 300 W for 30 min each; the solution after ultrasonic stirring is then poured into a 500 mL ball mill, and 500 g of 3 mm zirconia balls are added for ball milling. The ball milling process is as follows: the speed is 600 rpm, forward rotation for 18 min, stop for 2 min, reverse rotation for 18 min, and stop for 2 min; a total of 30 processes are repeated, and the total high-speed ball milling time is 20 h;
[0037] (3) First, the suspension obtained in step (2) is centrifuged at 4000 rpm, 1 / 2 of the upper suspension is collected and placed in a beaker, which is sealed and then continuously subjected to ice-water bath ultrasound for 10 hours, and the ice bag and water are replaced every 30 minutes to maintain the water temperature at 25°C. The mixed solution subjected to ice-water bath ultrasound is subjected to the first low-speed centrifugation to collect 1 / 2 of the upper suspension, wherein the low-speed centrifugation speed is 4000 rpm and the time is 8 minutes; then, the upper filtrate is subjected to the second high-speed centrifugation to collect 1 / 2 of the upper suspension to obtain an ultrathin MoS2 nanosheet solution, wherein the high-speed centrifugation speed is 10000 rpm and the time is 20 minutes; finally, the ultrathin MoS2 nanosheet solution is placed in a refrigerator for low-temperature freezing for 24 hours, and then placed in a freeze dryer for freeze-drying at -70°C for 72 hours to finally obtain ultrathin MoS2 nanosheets.
[0038] Figure 1 This is a SEM picture of molybdenum disulfide after hydrothermal synthesis in Example 1 of the present invention. It can be clearly seen that there are block agglomerates formed by stacking multiple MoS2 sheets over a large area, and the lateral size of a single MoS2 sheet is about 400-600nm;
[0039] Figure 2 This is a SEM picture of molybdenum disulfide after high-speed ball milling in Example 1 of the present invention. In the picture, MoS2 block agglomerates can still be seen, and there are some small flakes at the edge after exfoliation, and the size of which is about 300-500nm, which proves that the exfoliation effect of single high-speed ball milling is not obvious;
[0040] Figure 3This is an SEM picture of molybdenum disulfide after low-temperature freeze-drying in Example 1 of the present invention. It can be clearly seen that the MoS2 flakes in the picture are loosely stacked, the interlayer spacing is enlarged, the size of a single flake is about 250nm, and the peeling effect is good.
[0041] Embodiment 2:
[0042] The specific steps are as follows:
[0043] (1) Weigh 2 mmol of ammonium molybdate and 8 mmol of thiourea and dissolve them in 40 mL of deionized water and 30 mL of polyethylene glycol 200 to form a reaction solution. After stirring and ultrasonicating for 15 min each, transfer the mixture to a 100 mL reactor and react at 200° C. for 20 h. After the reaction is completed, naturally cool the mixture to room temperature. Filter the reaction product to obtain a black precipitate, wash it with deionized water and ethanol several times, and dry it in a vacuum drying oven at 70° C. for 8 h.
[0044] (2) The MoS2 powder synthesized in step (1) was mixed with deionized water and soapberry saponin in a mass ratio of 1:8:1 to obtain 50 g of a mixed solution, and the mixed solution was ultrasonicated and stirred at room temperature (25°C) for 30 min each at a power of 300 W; the solution after ultrasonic stirring was then poured into a 500 mL ball mill, and 500 g of 3 mm zirconia balls were added for ball milling. The ball milling process was as follows: the speed was 600 rpm, forward rotation for 18 min, stop for 2 min, reverse rotation for 18 min, and stop for 2 min; a total of 30 processes were repeated, and the total high-speed ball milling time was 20 h;
[0045] (3) First, the suspension obtained in step (2) is centrifuged at 4000 rpm, 1 / 2 of the upper suspension is collected and placed in a beaker, which is sealed and then continuously subjected to ice-water bath ultrasound for 10 hours, and the ice bag and water are replaced every 30 minutes to maintain the water temperature at 25°C. The mixed solution subjected to ice-water bath ultrasound is subjected to the first low-speed centrifugation to collect 1 / 2 of the upper suspension, wherein the low-speed centrifugation speed is 4000 rpm and the time is 8 minutes; then, the upper filtrate is subjected to the second high-speed centrifugation to collect 1 / 2 of the upper suspension to obtain an ultrathin MoS2 nanosheet solution, wherein the high-speed centrifugation speed is 10000 rpm and the time is 20 minutes; finally, the ultrathin MoS2 nanosheet solution is placed in a refrigerator for low-temperature freezing for 24 hours, and then placed in a freeze dryer for freeze drying at -70°C for 72 hours to finally obtain ultrathin MoS2 nanosheets.
[0046] Figure 4 This is a SEM picture of molybdenum disulfide after high-speed ball milling in Example 2 of the present invention. In the picture, the MoS2 block exists alone without agglomeration, but does not present a sheet-like stacking structure. This may be due to the low concentration of the surfactant, resulting in the interlayer van der Waals force not being destroyed;
[0047] Figure 5This is the SEM picture of molybdenum disulfide after low-temperature freeze-drying in Example 2 of the present invention. It can be clearly seen that after liquid ultrasonic treatment, the MoS2 block is peeled off into MoS2 flakes of different lateral sizes. The flake size is 100-500nm, and the peeling effect is more significant.
[0048] Embodiment 3:
[0049] The specific steps are as follows:
[0050] (1) Weigh 2 mmol of ammonium molybdate and 20 mmol of thioacetamide and dissolve them in 30 mL of deionized water and 30 mL of polyethylene glycol 400 to form a reaction solution. After stirring and ultrasonicating for 1.5 min each, transfer the mixture to a 100 mL reactor and react at 200° C. for 20 h. After the reaction is completed, naturally cool the mixture to room temperature. Filter the reaction product to obtain a black precipitate, wash it with deionized water and ethanol several times, and dry it in a vacuum drying oven at 70° C. for 8 h.
[0051] (2) The MoS2 powder synthesized in step (1) was mixed with deionized water, N-methylpyrrolidone and isopropanol in a mass ratio of 2:11:1:1 to obtain 50 g of a mixed solution, and the mixed solution was ultrasonicated and stirred at room temperature (25°C) for 30 min each at a power of 300 W; then the solution after ultrasonic stirring was poured into a 500 mL ball milling jar, and 500 g of 3 mm zirconia balls were added for ball milling. The ball milling process was as follows: the speed was 600 rpm, forward rotation for 18 min, stop for 2 min, reverse rotation for 18 min, and stop for 2 min; a total of 30 processes were repeated, and the total high-speed ball milling time was 20 h;
[0052] (3) First, the suspension obtained in step (2) is centrifuged at 4000 rpm, 1 / 2 of the upper suspension is collected and placed in a beaker, which is sealed and then continuously subjected to ice-water bath ultrasound for 10 hours, and the ice bag and water are replaced every 30 minutes to maintain the water temperature at 25°C. The mixed solution subjected to ice-water bath ultrasound is subjected to the first low-speed centrifugation to collect 1 / 2 of the upper suspension, wherein the low-speed centrifugation speed is 4000 rpm and the time is 8 minutes; then, the upper filtrate is subjected to the second high-speed centrifugation to collect 1 / 2 of the upper suspension to obtain an ultrathin MoS2 nanosheet solution, wherein the high-speed centrifugation speed is 10000 rpm and the time is 20 minutes; finally, the ultrathin MoS2 nanosheet solution is placed in a refrigerator for low-temperature freezing for 24 hours, and then placed in a freeze dryer for freeze drying at -70°C for 72 hours to finally obtain ultrathin MoS2 nanosheets.
[0053] Embodiment 4:
[0054] The specific steps are as follows:
[0055] (1) Weigh 2 mmol of ammonium molybdate tetrahydrate and 8 mmol of thioacetamide and dissolve them in 30 mL of deionized water and 30 mL of polyethylene glycol 400 to form a reaction solution. After stirring and ultrasonicating for 15 min each, transfer the mixture to a 100 mL reactor and react at 200 °C for 20 h. After the reaction is completed, naturally cool the mixture to room temperature. Filter the reaction product to obtain a black precipitate, wash it with deionized water and ethanol several times, and dry it in a vacuum drying oven at 70 °C for 8 h.
[0056] (2) The MoS2 powder synthesized in step (1) was mixed with deionized water, isopropanol and N-dimethylformamide in a mass ratio of 8:36:3:3 to obtain 50 g of a mixed solution, and the mixed solution was ultrasonicated and stirred at room temperature (25°C) for 30 min each at a power of 300 W; then the solution after ultrasonic stirring was poured into a 500 mL ball milling jar, and 500 g of 3 mm zirconia balls were added for ball milling. The ball milling process was as follows: the speed was 600 rpm, the forward rotation was 18 min, the stop was 2 min, the reverse rotation was 18 min, and the stop was 2 min; a total of 30 processes were repeated, and the total high-speed ball milling was 20 h;
[0057] (3) First, the suspension obtained in step (2) is centrifuged at 4000 rpm, 1 / 2 of the upper suspension is collected and placed in a beaker, which is sealed and then continuously subjected to ice-water bath ultrasound for 10 hours, and the ice bag and water are replaced every 30 minutes to maintain the water temperature at 25°C. The mixed solution subjected to ice-water bath ultrasound is subjected to the first low-speed centrifugation to collect 1 / 2 of the upper suspension, wherein the low-speed centrifugation speed is 4000 rpm and the time is 8 minutes; then, the upper filtrate is subjected to the second high-speed centrifugation to collect 1 / 2 of the upper suspension to obtain an ultrathin MoS2 nanosheet solution, wherein the high-speed centrifugation speed is 10000 rpm and the time is 20 minutes; finally, the ultrathin MoS2 nanosheet solution is placed in a refrigerator for low-temperature freezing for 24 hours, and then placed in a freeze dryer for freeze drying at -70°C for 72 hours to finally obtain ultrathin MoS2 nanosheets.
[0058] Application Example 1:
[0059] Compared with Example 2, it can be found that the ultra-thin MoS2 nanosheets obtained by using a higher mass ratio of soapberry saponin as the surfactant are more stable in morphology, and the lateral dimensions of the sheets are uniform without obvious stacking. Therefore, a certain amount of boric acid powder is dissolved in deionized water to obtain a 10.0% concentration of boric acid solution, and then the ultra-thin MoS2 nanosheets prepared in Example 1 are uniformly dispersed in a mixed solution of boric acid (BA) and water by ultrasonic dispersion to prepare a lubricating liquid, wherein the MoS2 concentration is 1.0%. The lubrication performance of the silicon nitride Si3N4 ball / silicon-doped diamond-like film disk friction pair is tested by using a UMT-5 rotary friction and wear tester. The experimental load is 3N and the rotation speed is 300rpm. The experimental results are as follows: Figure 6 shown.
[0060] It can be seen that the addition of ultra-thin MoS2 nanosheets has a certain effect of reducing wear and anti-wear. The friction coefficient drops from 0.025 to below 0.01. The wear surface of the silicon-doped diamond-like film disk is Figure 7 As shown, the surface wear marks are shallow and no obvious peeling marks are found.
[0061] 0.1 g of the ultrathin two-dimensional MoS2 nanosheets prepared in Example 1 was added to 10 g of a mixed solution of 30% propylene glycol (C3H8O3) and water and ultrasonically dispersed to form a lubricating liquid. The lubrication performance of the silicon nitride Si3N4 ball / sapphire friction pair was tested using a UMT-5 rotary friction and wear tester. The experimental load was 3N and the rotation speed was 300 rpm. The experimental results are shown in Figure 2. Figure 8 , 9 It was found that after adding nano-lubricating additives to the lubricant, the time to reach stable running-in was shortened to 1 / 4 of the original, and the friction coefficient was reduced to 0.008 after stable running-in.
[0062] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
Claims
1. A method for preparing ultrathin MoS2 nanosheets, characterized in that: include: S1, adding metal molybdenum salt and sulfur salt to a mixed solution of polyethylene glycol and deionized water, mixing evenly and sealing, and obtaining nano MoS2 by a hydrothermal synthesis method; S2, dispersing nano-MoS2 in a surfactant solution, and processing by high-speed ball milling to obtain a uniform MoS2 nanosheet suspension; S3, centrifuging the MoS2 nanosheet suspension, collecting 1 / 2 of the upper suspension and performing continuous ice-water bath sonication, centrifuging the mixed solution after ice-water bath sonication for the first time, collecting 1 / 2 of the upper filtrate and performing a second ice-water bath sonication, and collecting 1 / 2 of the upper filtrate by the second centrifugation to obtain an ultrathin MoS2 nanosheet solution; S4. Freeze the ultrathin MoS2 nanosheet solution in a refrigerator at below -25°C for 20-25 hours, and freeze-dry it in a freeze dryer at -70 to -80°C for three to four days to obtain ultrathin MoS2 nanosheets.
2. The method for preparing ultrathin MoS2 nanosheets according to claim 1, characterized in that: In step S1, the metal molybdenum salt includes one of sodium molybdate, ammonium molybdate, and ammonium molybdate tetrahydrate; the sulfur salt includes one of thiourea, L-cysteine, and thioacetamide; the molar ratio of the molybdenum element in the metal molybdenum salt to the sulfur element in the sulfur salt is 1: (4-10); the molecular weight of the polyethylene glycol is 200-800, wherein the mass fraction of the polyethylene glycol is 20wt%-60wt%, the mass fraction of deionized water is 40wt%-80wt%, and the sum of the mass fractions of the polyethylene glycol and the deionized water is 1; the temperature in the hydrothermal synthesis method is 180-220°C, and the reaction time is 18-24h.
3. The method for preparing ultrathin MoS2 nanosheets according to claim 1, characterized in that: In step S2, the surfactant includes at least one of soapberry saponin, N-methylpyrrolidone, isopropanol, and N-dimethylformamide.
4. The method for preparing ultrathin MoS2 nanosheets according to claim 1, characterized in that: In step S2, the mass ratio of nano-MoS2 and surfactant is (1-7): (1-7).
5. The method for preparing ultrathin MoS2 nanosheets according to claim 1, characterized in that: In step S2, the grinding balls used in the high-speed ball mill are 3 mm zirconia balls, the ball-to-material mass ratio is (5-20):1, the rotation speed is 400-600 rpm, and the ball milling time is 8-20 h.
6. The method for preparing ultrathin MoS2 nanosheets according to claim 1, characterized in that: In step S3, ultrasonic treatment is performed in an ice bath, and the ice pack and water are replaced every 30 minutes to maintain the water temperature at 25° C. The time is 8-12 hours, and the ultrasonic power is 220-300W.
7. The method for preparing ultrathin MoS2 nanosheets according to claim 1, characterized in that: In step S3, the first centrifugation speed is 3500-5000 rpm, and the time is 8-10 min; the second centrifugation speed is 10000-12000 rpm, and the time is 15-30 min.
8. An ultrathin MoS2 nanosheet, prepared by the preparation method described in any one of claims 1 to 7.
9. An application of an ultrathin MoS2 nanosheet prepared by the preparation method according to any one of claims 1 to 7, characterized in that: Ultrathin MoS2 nanosheets are applied in lubricants, including: using MoS2 nanosheets as acid liquid lubricant additives, and ultrathin MoS2 nanosheets as alcohol liquid lubricant additives; wherein the acid liquids include boric acid solution, citric acid solution, and oxalic acid solution; and the alcohol liquids include propylene glycol solution, 1-3 propylene glycol solution, and 1-4 butylene glycol solution.
10. The use of an ultrathin MoS2 nanosheet according to claim 9, characterized in that: The use concentration of ultrathin MoS2 nanosheets is 1.0wt%; when ultrathin MoS2 nanosheets are used as acid liquid lubricant additives, the friction pair is silicon nitride balls and silicon-doped diamond film disks; when ultrathin MoS2 nanosheets are used as alcohol liquid lubricant additives, the friction pair is silicon nitride balls and sapphire disks.
Citation Information
Patent Citations
Method for preparing liquid phase dispersion-based two-dimensional MoS2 nanosheets
CN103771517A
Method for preparing two-dimensional material nanosheet through ball-milling-enhanced stripping
CN110203896A
Method for hydro / solvothermal synthesis of multi-morphology nano molybdenum disulfide lubricating additive
CN115744990A