T2 / O2 / O3 type lithium ion battery positive electrode material as well as high-shear mixing spray drying preparation method and application of T2 / O2 / O3 type lithium ion battery positive electrode material
Preparation of lithium-ion battery positive electrode material through high shear mixed spray drying method solves the problem of limited control space of oxygen accumulation method in the prior art, realizes the preparation of multiple layered structures and excellent electrochemical performance, and is suitable for a wide range of electronics Products and power battery applications.
Patent Information
- Application Number
- CN202411033947.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The existing positive electrode materials of lithium-ion batteries have limited control space for oxygen accumulation in the layered structure, resulting in a single material configuration and poor electrochemical performance, which hinders the practical application of lithium-ion batteries.
The preparation method of high shear mixed spray drying is adopted to prepare the parent sodium ion layered oxide by high-temperature calcination method, and add it to the lithium salt solution for high shear homogenization to achieve Li+/Na+ ion exchange reaction, and obtain the Li+/Na+ ion exchange reaction. A lithium-ion battery cathode material with a layered structure of T2, O2 and O3.
This method can not only prepare lithium-polluted T2 phase layered structure and lithium-rich O2 phase layered structure, but also prepare thermodynamically stable O3 phase layered oxides. The material structure is stable, the electrochemical performance is excellent, and it is suitable for electronics Products and power battery market.
Smart Images

Figure CN118954628A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion battery positive electrode materials, and specifically relates to a T2 / O2 / O3 type lithium ion battery positive electrode material and a high shear mixing spray drying preparation method and application thereof. Background Art
[0002] Energy storage batteries are crucial to solving the energy and environmental problems facing human society. Among all types of batteries, lithium-ion batteries have been widely used in electric vehicles, portable electronic devices, robots and other power tools and electronic devices due to their high energy density and no memory effect. The invention of lithium battery technology also won the Nobel Prize in Chemistry in 2019. Among various lithium-ion battery components, the positive electrode occupies the highest cost and is expensive, which has a great impact on the cost and overall performance of lithium-ion batteries. Therefore, the development of the positive electrode is the key to the success of lithium-ion batteries. Lithium-ion battery positive electrode materials mainly include lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium iron phosphate (LiFePO4), ternary lithium nickel cobalt manganese oxide Li(Ni, Co, Mn)O2, etc. Lithium nickel cobalt manganese oxide Li(Ni, Co, Mn)O2 can be balanced and regulated in terms of specific energy, cyclability, safety and cost, and has received widespread attention.
[0003] However, due to the migration of transition metals (TMs) in the layered structure, the original layered structure degenerates into partially disordered oxides, causing serious and irreversible structural changes, resulting in severe voltage decay and poor rate performance, which hinders its practical application.
[0004] Therefore, improving the capacity and cycle performance of lithium-ion batteries by regulating the stacking arrangement of oxygen has become a research focus. However, the existing preparation methods of layered cathode materials mainly use the synthesis-coprecipitation method of the precursor and the subsequent high-temperature solid phase method, which generally obtains a stable O3-type layered oxide, and the space for regulating the oxygen stacking in the layered structure is limited. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a T2 / O2 / O3 type lithium-ion battery positive electrode material and its high-shear mixing spray drying preparation method and application, so as to solve the problem that the existing method cannot effectively regulate the oxygen accumulation mode in the layered structure, thereby resulting in the obtained material having a single configuration and poor electrochemical performance.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The invention discloses a high shear mixing spray drying preparation method for a T2 / O2 / O3 type lithium ion battery positive electrode material. The invention lies in combining high shear homogenization treatment with spray drying for the first time. The specific method includes:
[0008] Firstly, the parent sodium ion layered oxide Na was prepared by high temperature calcination method. m [Li x Ni y Co z Mn 1-x-y-z ]O2, then add it to the lithium salt solution, perform high shear homogenization to make the reaction materials mix evenly, then perform spray drying at 260-300°C, and then perform washing and drying to obtain the positive electrode material Na containing T2, O2 and O3 type layered structure. m [Li x Ni y Co z Mn 1-x-y-z ]O2; among which, 0.50≤m≤1.00, 0.00≤x≤0.33; 0.00≤y≤0.50; 0.00≤z≤0.50.
[0009] Preferably, the high shear mixing spray drying preparation method of the above-mentioned T2 / O2 / O3 type lithium ion battery positive electrode material specifically comprises the following steps:
[0010] 1) Weigh the raw materials
[0011] According to the chemical formula Na m [Li x Ni y Co z Mn 1-x-y-z ]O2 ratio, weigh the raw material transition metal oxide and sodium salt, mix them evenly; wherein, 0.50≤m≤1.00, 0.00≤x≤0.33; 0.00≤y≤0.50; 0.00≤z≤0.50;
[0012] 2) High temperature calcination
[0013] The mixed material in step 1) is calcined at high temperature and then cooled naturally to room temperature to obtain the parent sodium ion layered oxide Na m [Li x Ni y Co z Mn 1-x-y-z ]O2;
[0014] 3) High shear homogenization
[0015] The parent sodium ion layered oxide Na prepared in step 2) m [Li x Niy Co z Mn 1-x-y-z ]O2 is added to the lithium salt solution and subjected to high shear homogenization treatment to make it uniformly mixed to obtain a suspension;
[0016] 4) Spray drying
[0017] The suspension is spray-dried to obtain an ion-exchanged product, which is then washed and dried to obtain a T2 / O2 / O3 type lithium-ion battery cathode material, namely, a lithium-ion layered oxide Li m [Li x Ni y Co z Mn 1-x-y-z ]O2.
[0018] Further preferably, in step 1), the nickel-containing oxide is selected from NiO; the manganese-containing oxide is selected from MnO2, Mn3O4 or Mn2O3; the cobalt-containing oxide is selected from CoO, Co2O3 or Co3O4; and the Na salt is selected from Na2CO3, NaNO3, NaCl, NaCH3COO or NaOH.
[0019] Further preferably, in step 1), the mixing method includes ball milling, grinding, mechanical stirring, etc.;
[0020] Further preferably, in step 1), the molar ratio of the sodium salt to the transition metal oxide is 1:(1-1.5).
[0021] Further preferably, in step 2), the high temperature calcination treatment is carried out in an atmosphere of air at normal pressure, with the temperature being increased from room temperature to 800-850° C. at a heating rate of 3-10° C. / min, and the calcination is carried out for 8-12 hours.
[0022] Specifically, the sample mixed in step 1) is placed in a muffle furnace and subjected to high-temperature calcination treatment in normal pressure and air atmosphere.
[0023] Further preferably, in step 3), according to Li + and Na + The molar ratio of the reaction material matrix sodium ion layered oxide Na is 1: (1.2 to 1:5) m [Li x Ni y Co z Mn 1-x-y-z ]O2 and prepare lithium salt solution;
[0024] The lithium salt solution is prepared by mixing lithium salt and water, or a mixture of lithium salt and potassium salt and water in a dosage ratio of 1 g: (10-30) mL; wherein:
[0025] Li in mixed salt of lithium salt and potassium salt+ and K + The molar ratio is (0.2-1.0):1;
[0026] The lithium salt is selected from LiNO3, LiOH, Li2CO3, LiCH3COO or LiCl;
[0027] The potassium salt is selected from KNO3, K2CO3, or KCl.
[0028] Furthermore, the water is deionized water.
[0029] Further preferably, in step 3), the high shear homogenization treatment uses a high shear homogenizer, the speed is set to 6000-10000 rpm, and the treatment time is 30-60 min.
[0030] Further preferably, in step 4), the spray drying temperature is 260-300° C., the feed rate is 10-20 rpm, and the needle passing frequency is set to 5-10 s.
[0031] Furthermore, in step 4), after obtaining the product after ion exchange, it is first filtered or centrifuged, and then the impurities generated by the reaction are washed away with deionized water, and washed with anhydrous ethanol 2 to 3 times, and the obtained product is dried and collected.
[0032] The present invention also discloses a T2 / O2 / O3 type lithium ion battery positive electrode material prepared by the above-mentioned high-shear mixed spray drying preparation method, including an O3 type lithium ion battery positive electrode material with a stable structure, a T2 type lithium ion battery positive electrode material with a metastable structure or an O2 type lithium ion battery positive electrode material with a metastable structure, and a lithium ion battery positive electrode material with a T2 / O2 and O2 / O3 composite phase layered structure; the above-mentioned lithium ion battery positive electrode material is composed of micron single crystal particles, the grain size distribution is between 5 and 20 microns, and the particle size is controllable.
[0033] The present invention also discloses the application of the above-mentioned T2 / O2 / O3 type lithium ion battery positive electrode material in the preparation of lithium ion batteries. The capacity retention rate of the T2 / O2 / O3 type lithium ion battery positive electrode material reaches more than 90% after 50 cycles. The prepared LCO has a capacity of 210mAh / g under the conditions of 3-4.6V and 1C, and the capacity retention rate reaches 90% after 50 cycles.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] The invention discloses a method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery. The invention lies in that a high-shear mixed spray drying method is used to firstly synthesize a sodium-containing layered oxide material by a high-temperature solid phase method (i.e., by high-temperature calcination treatment), and then the layered oxide material is immersed in a lithium salt solution, and the two are mixed evenly by a high-shear homogenization treatment to obtain a uniform suspension, and finally the Li + / Na + Ion exchange reaction to obtain different structure layered oxides (Li m [Li x Ni y Co z Mn 1-x-y-z ]O2). The method of the present invention can not only prepare a lithium-poor T2 phase layered structure, but also prepare a lithium-rich metastable O2 phase layered structure and a thermodynamically stable O3 phase layered oxide. In addition, the method can also prepare T2 / O2, T2 / O2 / O3 and O2 / O3 composite phase structure layered oxides. The method is simple in process, easy to operate, and has a stable and reliable material structure. m [Li x Ni y Co z Mn 1-x-y-z ]O2 is used as a template to effectively prepare lithium-ion battery positive electrode materials with different layered structures, which is convenient for industrial promotion.
[0036] Furthermore, compared with the traditional solid phase reaction method, this method can prepare O2, O3 and O2 / O3 type layered oxides by adjusting the reaction temperature of spray drying;
[0037] Furthermore, for Li + and Na + The T2-type layered cathode material can be prepared by regulating the ratio of Li and the concentration of Li salt.
[0038] Furthermore, by regulating the feed rate, the crystal particle size can be effectively controlled, and the size distribution is uniform, between 5 and 20 microns.
[0039] The layered positive electrode material prepared by the method of the present invention has unique structural characteristics and excellent electrochemical properties. The oxide particles are all composed of micron-sized single crystal particles, the grain size distribution is between 5 and 20 microns, the particle size is controllable, the batch uniformity is good, the consistency is good, it has excellent cycle stability, and the application range is wide (4.3 to 4.8V), so it can be widely used in the electronic products and power battery markets. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is the X-ray diffraction spectrum of the O2-type layered positive electrode material prepared in Example 1 of the present invention;
[0041] Figure 2 The first charge-discharge curve of the O2-type layered cathode material prepared in Example 1 of the present invention at a rate of 0.1C;
[0042] Figure 3 This is the X-ray diffraction spectrum of the O3-type layered positive electrode material prepared in Example 2 of the present invention;
[0043] Figure 4 The cycle performance of the O3-type layered positive electrode material prepared in Example 2 of the present invention;
[0044] Figure 5 This is a scanning electron microscope image of the O2-type layered positive electrode material prepared in Example 3 of the present invention;
[0045] Figure 6 This is the X-ray diffraction spectrum of the O2-type layered positive electrode material prepared in Example 3 of the present invention;
[0046] Figure 7 This is the X-ray diffraction spectrum of the O2-type layered positive electrode material prepared in Example 4 of the present invention;
[0047] Figure 8 This is a scanning electron microscope image of the O2-type layered positive electrode material prepared in Example 4 of the present invention;
[0048] Fig. 9 This is the X-ray diffraction spectrum of the O2-type layered positive electrode material prepared in Example 5 of the present invention;
[0049] Fig.10 This is a scanning electron microscope image of the O2-type layered positive electrode material prepared in Example 5 of the present invention;
[0050] Fig.11 This is the X-ray diffraction spectrum of the T2-type layered positive electrode material prepared in Example 6 of the present invention;
[0051] Fig.12 The cycle performance of the T2-type layered positive electrode material prepared in Example 6 of the present invention;
[0052] Fig.13 This is the X-ray diffraction spectrum of the T2-type layered positive electrode material prepared in Example 7 of the present invention. DETAILED DESCRIPTION
[0053] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0054] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0055] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0056] Example 1
[0057] In this embodiment, according to the chemical formula Li[Li 0.2 Ni 0.2 Co 0.1 Mn 0.5 ]O2 ingredients.
[0058] A method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery comprises the following steps:
[0059] Step 1. Weighing:
[0060] Weigh the corresponding Na2CO3, LiOH, NiO, Co3O4 and Mn2O3 according to the molar ratio of sodium, lithium, nickel, cobalt and manganese elements of 10:2:2:1:5, grind them in a mortar and mix them evenly.
[0061] Step 2. Calcination:
[0062] The mixed materials were heated to 800°C at a rate of 5°C / min in an atmosphere of air at normal pressure, kept at this temperature for 12 h, and naturally cooled to room temperature to obtain a P2-type sodium-containing layered oxide Na[Li 0.2 Ni 0.2 Co 0.1 Mn 0.5 ]O2.
[0063] Step 3. High Shear:
[0064] Weigh LiNO3 with a specific content and dissolve it in deionized water, the ratio of LiNO3 to deionized water is 1:20g / ml, and prepare a lithium salt solution. Weigh the prepared P2 type sodium ion layered oxide according to the molar ratio of lithium to sodium element of 1:1.2, add it to the prepared Li salt solution, and mix it evenly using a high shear homogenizer at a speed of 8000rpm for 30min.
[0065] Step 4. Spray drying:
[0066] The mixed suspension was spray dried at a temperature of 280°C, a feed rate of 10 rpm, a needle frequency of 5s, and a wind speed of 100%. The ion exchange product was obtained in the receiver. The obtained product was filtered or centrifuged, and the impurities produced by the reaction were washed with deionized water, and washed with ethanol for 2 to 3 times. The obtained product was dried and collected to obtain the lithium ion layered oxide Li[Li 0.2 Ni 0.2 Co 0.1 Mn 0.5 ]O2.
[0067] The charging and discharging performance test process of the positive electrode material prepared in this embodiment is as follows:
[0068] The electrochemical performance tests conducted by the present invention all used self-assembled CR2032 button batteries;
[0069] Weigh a certain amount of the positive electrode material, acetylene black, and binder polyvinylidene fluoride (PVDF) prepared in this embodiment in a mass ratio of 8:1:1, add them to N-methylpyrrolidone (NMP) to make a slurry. The content of NMP is 30 times that of PVDF. Evenly coat it on aluminum foil, vacuum dry it at 80°C for 12 hours, and then cut it into pole pieces with a diameter of 12 mm using a mold; the metal lithium sheet is used as the negative electrode, Celgard 2400 commercial polypropylene film is used as the diaphragm, and the electrolyte is 1M LiPF6 EC / DEC (1:1) solution. The battery is assembled in an argon-filled glove box. After standing for 10 hours, the electrochemical performance test of the battery was carried out at a voltage range of 2.0~4.8V and 0.1C. The results show that the Li[Li prepared in this embodiment 0.2 Ni 0.2 Co 0.1 Mn 0.5 ]O2 is the O2 structure, such as Figure 1 As shown, its first discharge capacity at 0.1C rate is more than 200mAh / g ( Figure 2 ).
[0070] Example 2
[0071] In this embodiment, according to the chemical formula Li[Li 0.2 Ni 0.2 Mn 0.6 ]O2 ingredients.
[0072] A method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery comprises the following steps:
[0073] Step 1. Weighing:
[0074] Weigh the corresponding Na2CO3, LiOH, NiO, and Mn3O4 according to the molar ratio of sodium, lithium, nickel, and manganese elements of 5:1:1:3, grind them in a ball mill, and mix them evenly.
[0075] Step 2. Calcination:
[0076] The mixed materials were heated to 800°C at a heating rate of 5°C / min in an atmosphere of air at normal pressure, kept at this temperature for 12 h, and naturally cooled to room temperature to obtain P2-type sodium ion layered oxide Na[Li 0.2 Ni 0.2 Mn 0.6 ]O2.
[0077] Step 3. High Shear:
[0078] Weigh LiNO3 with a specific content and dissolve it in deionized water, the ratio of LiNO3 to deionized water is 1:20g / ml, and prepare a lithium salt solution. Weigh the prepared P2 type sodium ion layered oxide according to the molar ratio of lithium to sodium element of 1:1.2, add it to the prepared Li salt solution, and mix it evenly using a high shear homogenizer at a speed of 8000rpm for 30min.
[0079] Step 4. Spray drying:
[0080] The mixed suspension was spray dried at a temperature of 300°C, a feed rate of 10 rpm, a needle frequency of 5s, and a wind speed of 100%. The ion exchange product was obtained in the receiver. The obtained product was filtered or centrifuged, and the impurities generated by the reaction were washed with deionized water, and washed with ethanol for 2 to 3 times. The obtained product was dried and collected to obtain the lithium ion layered oxide Li[Li 0.2 Ni 0.2 Mn 0.6 ]O2.
[0081] The layered oxide Li[Li 0.2 Ni 0.2 Mn 0.6 ]XRD of O2 Figure 3 , it can be seen from the figure that all the diffraction peaks belong to the O3 type layered structure.
[0082] The charge and discharge performance test of the positive electrode material prepared in this embodiment: The test method is the same as that in Example 1. The results show that the first discharge capacity of the O3 type lithium ion layered positive electrode material prepared in this embodiment at 0.1C is 214mAh / g. After 50 cycles, the capacity retention rate is 98%. Figure 4 .
[0083] Example 3
[0084] In this embodiment, the ingredients are prepared according to the chemical formula LiCoO2.
[0085] A method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery comprises the following steps:
[0086] Step 1. Weighing:
[0087] Weigh the corresponding Na2CO3 and Co3O4 according to the molar ratio of sodium to cobalt element of 1:1, grind them in a ball mill and mix them evenly.
[0088] Step 2. Calcination:
[0089] The uniformly mixed material was heated to 800°C at a heating rate of 5°C / min in an air atmosphere at normal pressure, kept at that temperature for 12 hours, and naturally cooled to room temperature to obtain a P2 type sodium ion layered oxide NaCoO2.
[0090] Step 3. High Shear:
[0091] Weigh LiNO3 with a specific content and dissolve it in deionized water, the ratio of LiNO3 to deionized water is 1:20g / ml, and prepare a lithium salt solution. Weigh the prepared P2 type sodium ion layered oxide according to the molar ratio of lithium to sodium element of 1:1.2, add it to the prepared Li salt solution, and mix it evenly using a high shear homogenizer at a speed of 8000rpm for 30min.
[0092] Step 4. Spray drying:
[0093] The mixed suspension is spray dried at a temperature of 280°C, a feed rate of 10rpm, a needle frequency of 5s, and a wind speed of 100%, and the ion exchange product is obtained in the receiver. The obtained product is filtered or centrifuged, and the impurities generated by the reaction are washed with deionized water, and washed with ethanol 2 to 3 times. The product is dried and collected to obtain the lithium ion layered oxide LiCoO2.
[0094] The morphology of LiCoO2 prepared in this example is shown in Figure 5 From the figure, it can be seen that the prepared layered oxide is a single crystal particle with a uniform particle size distribution of 9 μm and a flake structure. The XRD diagram shows that it is an O2 structure. Figure 6 .
[0095] Charge and discharge performance test: The test method is the same as that in Example 1. The results show that the first discharge capacity of the positive electrode material prepared in this example at 1C reaches 193 mAh / g.
[0096] Example 4
[0097] In this embodiment, the ingredients are prepared according to the chemical formula LiCoO2.
[0098] A method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery comprises the following steps:
[0099] Step 1. Weighing:
[0100] Weigh the corresponding Na2CO3 and Co3O4 according to the molar ratio of sodium to cobalt element of 1:1, grind them in a ball mill and mix them evenly.
[0101] Step 2. Calcination:
[0102] The uniformly mixed material was heated to 800°C at a heating rate of 5°C / min in an air atmosphere at normal pressure, kept at that temperature for 12 hours, and naturally cooled to room temperature to obtain a P2 type sodium ion layered oxide NaCoO2.
[0103] Step 3. High Shear:
[0104] Weigh LiNO3 with a specific content and dissolve it in deionized water, the ratio of LiNO3 to deionized water is 1:20g / ml, and prepare a lithium salt solution. Weigh the prepared P2 type sodium ion layered oxide according to the molar ratio of lithium to sodium element of 1:1.2, add it to the prepared Li salt solution, and mix it evenly using a high shear homogenizer at a speed of 8000rpm for 30min.
[0105] Step 4. Spray drying:
[0106] The mixed suspension is spray dried at a temperature of 280°C, a feed rate of 15rpm, a needle frequency of 5s, and a wind speed of 100%, and the ion exchange product is obtained in the receiver. The obtained product is filtered or centrifuged, and the impurities generated by the reaction are washed with deionized water, and washed with ethanol 2 to 3 times. The product obtained is dried and collected, which is the lithium ion layered oxide LiCoO2.
[0107] The XRD pattern of LiCoO2 prepared in this example is shown in Figure 7From the figure, it can be seen that LiCoO2 is an O2 structure. The O2 type lithium ion layered oxide particles prepared in this embodiment have a size of about 6 μm. Figure 8 .
[0108] Charge and discharge performance test: The test method is the same as that of Example 1. The first discharge capacity of the positive electrode material prepared in this example at 1C is 210 mAh / g.
[0109] Example 5
[0110] In this embodiment, the ingredients are prepared according to the chemical formula LiCoO2.
[0111] A method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery comprises the following steps:
[0112] Step 1. Weighing:
[0113] Weigh the corresponding salts and oxides such as Na2CO3 and Co3O4 according to the molar ratio of sodium to cobalt elements of 1:1, grind them in a ball mill and mix them evenly.
[0114] Step 2. Calcination:
[0115] The uniformly mixed material was heated to 800°C at a heating rate of 5°C / min in an air atmosphere at normal pressure, kept at that temperature for 12 hours, and naturally cooled to room temperature to obtain a P2 type sodium ion layered oxide NaCoO2.
[0116] Step 3. High Shear:
[0117] Weigh LiNO3 with a specific content and dissolve it in deionized water, the ratio of LiNO3 to deionized water is 1:20g / ml, and prepare a lithium salt solution. Weigh the prepared P2 type sodium ion layered oxide according to the molar ratio of lithium to sodium element of 1:1.2, add it to the prepared Li salt solution, and mix it evenly using a high shear homogenizer at a speed of 8000rpm for 30min.
[0118] Step 4. Spray drying:
[0119] The mixed suspension is spray dried at a temperature of 280°C, a feed rate of 20rpm, a needle frequency of 5s, and a wind speed of 100%, and the ion exchange product is obtained in the receiver. The obtained product is filtered or centrifuged, and the impurities generated by the reaction are washed with deionized water, and washed with ethanol 2 to 3 times. The product obtained is dried and collected, which is the lithium ion layered oxide LiCoO2.
[0120] The XRD pattern of LiCoO2 prepared in this example is shown in Fig. 9From the figure, it can be seen that LiCoO2 is an O2 structure. The O2 type lithium ion layered oxide particles prepared in this embodiment have a size of about 4 μm. Fig.10 .
[0121] Charge and discharge performance test: The test method is the same as that of Example 1. The first discharge capacity of the positive electrode material prepared in this example at 1C is 203 mAh / g.
[0122] Example 6
[0123] In this embodiment, according to the chemical formula Li[Li 0.2 Ni 0.2 Co 0.1 Mn 0.5 ]O2 ingredients.
[0124] A method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery comprises the following steps:
[0125] Step 1. Weighing:
[0126] Weigh the corresponding Na2CO3, LiOH, NiO, Co3O4, and Mn2O3 according to the molar ratio of sodium, lithium, nickel, cobalt, and manganese elements of 10:2:2:1:5, grind them in a ball mill, and mix them evenly.
[0127] Step 2. Calcination:
[0128] The mixed materials were heated to 800°C at a heating rate of 5°C / min in an atmosphere of air at normal pressure, kept at this temperature for 12 h, and naturally cooled to room temperature to obtain P2-type sodium ion layered oxide Na[Li 0.2 Ni 0.2 Co 0.1 Mn 0.5 ]O2.
[0129] Step 3. High Shear:
[0130] Weigh LiNO3 with a specific content and dissolve it in deionized water, the ratio of LiNO3 to deionized water is 1:20g / ml, and prepare a lithium salt solution. Weigh the prepared P2 type sodium ion layered oxide according to the molar ratio of lithium to sodium element of 1:1.5, add it to the prepared Li salt solution, and mix it evenly using a high shear homogenizer at a speed of 8000rpm for 30min.
[0131] Step 4. Spray drying:
[0132] The mixed suspension was spray dried at a temperature of 280°C, a feed rate of 10 rpm, a needle frequency of 5s, and a wind speed of 100%. The ion exchange product was obtained in the receiver. The obtained product was filtered or centrifuged, and the impurities produced by the reaction were washed with deionized water, and washed with ethanol for 2 to 3 times. The obtained product was dried and collected to obtain the lithium ion layered oxide Li[Li 0.2 Ni 0.2 Co 0.1 Mn 0.5 ]O2.
[0133] The Li[Li 0.2 Ni 0.2 Co 0.1 Mn 0.5 ]XRD of O2 Fig.11 From the figure, we can see that all the diffraction peaks belong to the T2 layered structure, and the space group is Cmca.
[0134] Charge and discharge performance test: The test method is the same as that of Example 1. The results show that the positive electrode material prepared in this example has an initial discharge capacity of 204 mAh / g at a 1C rate, and the capacity is still 195 mAh / g after 50 cycles. Fig.12 .
[0135] Example 7
[0136] In this embodiment, according to the chemical formula Li[Li 0.2 Ni 0.2 Co 0.1 Mn 0.5 ]O2 ingredients.
[0137] A method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery comprises the following steps:
[0138] Step 1. Weighing:
[0139] Weigh the corresponding Na2CO3, LiOH, NiO, Co3O4, and Mn2O3 according to the molar ratio of sodium, lithium, nickel, cobalt, and manganese elements of 10:2:2:1:5, grind them in a ball mill, and mix them evenly.
[0140] Step 2. Calcination:
[0141] The mixed materials were heated to 800°C at a heating rate of 5°C / min in an air atmosphere at normal pressure, kept at this temperature for 12 h, and naturally cooled to room temperature to obtain P2-type sodium ion layered oxide Na[Li 0.2 Ni 0.2 Co 0.1 Mn 0.5 ]O2.
[0142] Step 3. High Shear:
[0143] Weigh LiNO3 with a specific content and dissolve it in deionized water, the ratio of LiNO3 to deionized water is 1:30g / ml, and prepare a lithium salt solution. Weigh the prepared P2 type sodium ion layered oxide according to the molar ratio of lithium to sodium element of 1:1.2, add it to the prepared Li salt solution, and mix it evenly using a high shear homogenizer at a speed of 8000rpm for 30min.
[0144] Step 4. Spray drying:
[0145] The mixed suspension was spray dried at a temperature of 280°C, a feed rate of 10 rpm, a needle frequency of 5s, and a wind speed of 100%. The ion exchange product was obtained in the receiver. The obtained product was filtered or centrifuged, and the impurities produced by the reaction were washed with deionized water, and washed with ethanol for 2 to 3 times. The obtained product was dried and collected to obtain the lithium ion layered oxide Li[Li 0.2 Ni 0.2 Co 0.1 Mn 0.5 ]O2.
[0146] The Li[Li 0.2 Ni 0.2 Co 0.1 Mn 0.5 ]XRD of O2 Fig.13 From the figure, we can see that all the diffraction peaks belong to the T2 layered structure, and the space group is Cmca.
[0147] Charge and discharge performance test: The test method is the same as that in Example 1. The results show that the first discharge capacity of the positive electrode material prepared in this example at 1C is 208 mAh / g.
[0148] It can be seen that the present invention considers ion exchange technology as a powerful method for obtaining metastable materials with advanced energy storage functions, which can not only produce various T2, O2 and O3 type layered structures, but also these layered positive electrode materials have unique structural stability and excellent electrochemical performance. Among them, the oxygen stacking order and coordination environment of alkali metals and the composition of lithium-containing oxides can be predicted and adjusted by adjusting the parent Na-based precursor. Therefore, the ion exchange strategy can achieve efficient preparation of lithium-ion ternary positive electrode materials, which is conducive to industrial implementation. The method of the present invention can not only prepare thermodynamically stable O3 phase layered oxides, but also can prepare metastable T2 and O2 phase layered structures, and the prepared oxide particles are all composed of micron-sized single crystal particles, the grain size distribution is between 5 and 10 microns, the particle size is controllable, the consistency is good, it has excellent cycle stability, and a wide range of use (4.3 to 4.8V), which can be widely used in the electronic products and power vehicle markets. At the same time, it can be seen from the performance test results that the lithium-ion battery positive electrode material LiTMO2 prepared by the present invention has excellent cycle performance. Under the conditions of 2.0-4.8V and 0.1C, the capacity retention rate of the NCM material after 50 cycles is still as high as 90% or more; the prepared LCO has a capacity of up to 210mAh / g under the conditions of 3-4.6V and 1C, and the capacity retention rate of the material after 50 cycles is as high as 90%. Therefore, the present invention is generally applicable to various layered lithium-embedded oxides with ideal structures and morphologies, and provides potential opportunities for the design and development of lithium-ion battery positive electrodes.
[0149] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A high shear mixing spray drying method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery, characterized in that: include: Firstly, the parent sodium ion layered oxide Na was prepared by high temperature calcination method. m [Li x Ni y Co z Mn 1-x-y-z ]O2, then add it to the lithium salt solution, perform high shear homogenization to make the reaction materials mix evenly, then perform spray drying at 260-300°C, and then perform washing and drying to obtain the positive electrode material Na containing T2, O2 and O3 type layered structure. m [Li x Ni y Co z Mn 1-x-y-z ]O2; among which, 0.50≤m≤1.00, 0.00≤x≤0.33; 0.00≤y≤0.50; 0.00≤z≤0.
50.
2. The high shear mixing spray drying method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery according to claim 1, characterized in that: The following steps are involved: 1) According to the chemical formula Na m [Li x Ni y Co z Mn 1-x-y-z ]O2 ratio, take the raw material transition metal oxide and sodium salt, mix them evenly; wherein, 0.50≤m≤1.00, 0.00≤x≤0.33; 0.00≤y≤0.50; 0.00≤z≤0.50; 2) The mixed material in step 1) is calcined at high temperature, and then cooled naturally to room temperature to obtain the parent sodium ion layered oxide Na m [Li x Ni y Co z Mn 1-x-y-z ]O2; 3) the parent sodium ion layered oxide Na prepared in step 2) m [Li x Ni y Co z Mn 1-x-y-z ]O2 is added to the lithium salt solution and subjected to high shear homogenization treatment to make it uniformly mixed to obtain a suspension; 4) The suspension is spray-dried to obtain an ion-exchanged product, which is then washed and dried to obtain a T2 / O2 / O3 type lithium-ion battery positive electrode material, i.e., a lithium-ion layered oxide Li m [Li x Ni y Co z Mn 1-x-y-z ]O2.
3. The high shear mixing spray drying method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery according to claim 2, characterized in that: In step 1), the transition metal oxide includes nickel-containing oxide, manganese-containing oxide and cobalt-containing oxide; wherein: The nickel-containing oxide is selected from NiO; the manganese-containing oxide is selected from MnO2, Mn3O4 or Mn2O3; the cobalt-containing oxide is selected from CoO, Co2O3 or Co3O4; the Na salt is selected from Na2CO3, NaNO3, NaCl, NaCH3COO or NaOH.
4. The high shear mixing spray drying method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery according to claim 2, characterized in that: In step 1), the molar ratio of the sodium salt to the transition metal oxide is 1:(1-1.5).
5. The high shear mixing spray drying method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery according to claim 2, characterized in that: In step 2), the high temperature calcination treatment is carried out in an atmosphere of air at normal pressure, with the temperature being raised from room temperature to 800-850° C. at a heating rate of 3-10° C. / min, and the calcination is carried out for 8-12 hours.
6. The high shear mixing spray drying method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery according to claim 2, characterized in that: In step 3), according to Li + and Na + The reaction material matrix sodium ion layered oxide Na is weighed at a molar ratio of 1: (1.2-1.5) m [Li x Ni y Co z Mn 1-x-y-z ]O2 and prepare a lithium salt solution; the lithium salt solution is prepared by mixing lithium salt or a mixed salt of lithium salt and potassium salt with deionized water in a dosage ratio of 1g: (10-30)mL; wherein: Li in mixed salt of lithium salt and potassium salt + and K + The molar ratio is (0.2-1.0):1; The lithium salt is selected from LiNO3, LiOH, Li2CO3, LiCH3COO or LiCl; The potassium salt is selected from KNO3, K2CO3, or KCl.
7. The high shear mixing spray drying method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery according to claim 2, characterized in that: In step 3), the high shear homogenization treatment uses a high shear homogenizer, the speed is set to 6000-10000 rpm, and the treatment time is 30-60 min.
8. The high shear mixing spray drying method for preparing a positive electrode material for a T2 / O2 / O3 type lithium ion battery according to claim 2, characterized in that: In step 4), the spray drying temperature is 260-300° C., the feed rate is 10-20 rpm, and the needle passing frequency is set to 5-10 s.
9. A T2 / O2 / O3 type lithium ion battery positive electrode material prepared by the high shear mixing spray drying preparation method according to any one of claims 1 to 8, characterized in that: T2 / O2 / O3 type lithium-ion battery positive electrode materials include O3 type lithium-ion battery positive electrode materials with a stable structure, T2 type lithium-ion battery positive electrode materials with a metastable structure or O2 type lithium-ion battery positive electrode materials with a metastable structure, and lithium-ion battery positive electrode materials with T2 / O2, T2 / O2 / O3 and O2 / O3 composite phase layered structures; the above lithium-ion battery positive electrode materials are composed of micron single crystal particles, the grain size distribution is between 5 and 20 microns, and the particle size is controllable.
10. Use of the T2 / O2 / O3 type lithium ion battery positive electrode material according to claim 9 in the preparation of lithium ion batteries, characterized in that: The capacity retention rate of the T2 / O2 / O3 type lithium ion battery positive electrode material after 50 cycles is more than 90%; the prepared LCO has a capacity of 210mAh / g under the conditions of 3-4.6V and 1C, and the capacity retention rate after 50 cycles is 90%.
Citation Information
Patent Citations
Layered cobalt-free manganese-based lithium ion battery positive electrode material as well as preparation method and application thereof
CN114242969A
T2 type lithium cobalt oxide positive electrode material with space group of Cmca and preparation method of T2 type lithium cobalt oxide positive electrode material
CN114784269A
Single-crystal lithium ion battery positive electrode material with different layered structures as well as preparation method and application of single-crystal lithium ion battery positive electrode material
CN114956210A
Nanoscale high-entropy phosphate material as well as preparation method and application thereof
CN116692809A
Method for producing positive electrode active material
JP2022097885A
Cited By
Positive electrode material, electrochemical device, and electronic device
WO2026174429A1