Preparation method of metakaolin-based phosphate geopolymer

By using a combination of metakaolin, phosphate solution and magnesium oxide, rapid coagulation and curing of acid-excited polymers is achieved at room temperature, solving the problem of high energy consumption in the prior art, and is suitable for practical engineering applications.

CN118955035APending Publication Date: 2024-11-15HUNAN GUIYE TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411059430.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-03
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing acid-excited polymers are difficult to cure at room temperature and require heating operation, resulting in high energy consumption and are not conducive to actual engineering applications.

Method used

Metakaolin and phosphate solutions are used as raw materials, magnesium oxide is added, and the synthesis and curing of polymers are achieved by standing curing at room temperature to avoid heating operations.

Benefits of technology

The rapid condensation and curing of ground polymers is achieved under room temperature, saving energy, reducing production costs, and the process is simple, safe and environmentally friendly, suitable for practical engineering applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a preparation method of a metakaolin-based phosphate geopolymer. The preparation method comprises the following steps: taking metakaolin and a phosphate solution as raw materials, adding magnesium oxide, and uniformly stirring; and standing and curing at room temperature to a preset age. The metakaolin and the phosphate solution are used as reaction raw materials, the magnesium oxide additive is added, synthesis and curing forming of the geopolymer at the room temperature are achieved, heating operation is not needed, the process is simple, a large amount of energy can be saved, and engineering application is easy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of geopolymer preparation, and specifically relates to a method for preparing a metakaolin-based phosphate geopolymer. Background Art

[0002] As traditional silicate cement production has high energy consumption and high resource consumption, as well as environmental pollution, the exploration and development of low-energy, environmentally friendly building materials has become a hot spot and highlight in the global research of green building materials. Geopolymers are considered to be a green and low-carbon cementitious material with great potential, which has attracted widespread attention and research interest from many scholars around the world. At present, the preparation and performance research of alkali-activated geopolymers is relatively mature and has been successfully used in production practice, but the research on acid-activated geopolymers has yet to be carried out.

[0003] The reaction of acidic phosphate and iron / aluminum silicate materials is a slow solidification process at room temperature, which takes several days to harden. The most commonly used solution at present is to heat up and cure. The prepared geopolymer is placed in an environment of 40-80℃ for curing for 2-10 hours, so that it can be quickly molded and demolded to meet the use requirements. However, heating and curing consumes a lot of energy, is inconvenient to operate, and is not conducive to the application of actual engineering. Therefore, various shaping accelerators are generally used to achieve rapid shaping and demolding in a short time and reduce energy consumption.

[0004] Chinese patent CN101560071A discloses a phosphate-based geopolymer porous material and a preparation method thereof, which uses metakaolin, alumina (or aluminum hydroxide), phosphoric acid and water as raw materials, and aluminum powder as a foaming agent, and foams at a temperature of 50-90°C to prepare a porous material with a geopolymer material as a skeleton and good performance. The prepared slurry is placed at room temperature for 0-24 hours, and then placed in a 50-90°C constant temperature box for curing for 2-8 hours to accelerate the curing and molding of the geopolymer. This process will generate a certain amount of energy consumption, and the temperature has a greater impact on the molding and strength development of the geopolymer slurry, which is difficult to control.

[0005] Phosphoaluminosilicate inorganic polymers activated by phosphoric acid have obvious disadvantages such as difficulty in curing at room temperature and high heat release. Although a large number of literature and practical experience have shown that temperature curing can accelerate the polymerization reaction of acid-activated geopolymers, the actual engineering application background limits the curing method during the preparation of the geopolymer. Therefore, the working performance, setting time and early strength of acid-activated geopolymers in actual engineering environments are issues that must be solved in actual engineering applications. Summary of the invention

[0006] Therefore, the present application provides a method for preparing a metakaolin-based phosphate geopolymer, which can solve the problem of high energy consumption in preparing geopolymers in the prior art.

[0007] In order to solve the above problems, the present application provides a method for preparing a metakaolin-based phosphate geopolymer, comprising:

[0008] Take metakaolin and phosphate solution as raw materials, add magnesium oxide, stir evenly; let stand and cure at room temperature until the preset age.

[0009] In some embodiments,

[0010] The method also includes: preparing the phosphate solution: mixing the phosphoric acid solution with aluminum hydroxide, and aging the mixture for a preset period of time.

[0011] In some embodiments,

[0012] The molar ratio of phosphoric acid to aluminum hydroxide in the phosphoric acid solution is set to 2-4:1.

[0013] In some embodiments,

[0014] The mass percentage concentration of the phosphoric acid solution is set to 75-85%, and the mass percentage concentration of the prepared phosphate solution is 50-60%.

[0015] In some embodiments,

[0016] The preset time period is set to 18-30 hours.

[0017] In some embodiments,

[0018] The percentage of magnesium oxide to the mass of the metakaolin is set to m, and 0% <m≤3%。

[0019] In some embodiments,

[0020] The molar ratio of the metakaolin to the phosphate solution is set to Al:P=0.36-0.40:1.01-1.10.

[0021] In some embodiments,

[0022] The magnesium oxide and the metakaolin are mixed and stirred, the phosphate solution is added dropwise during the stirring process, and the mixture is allowed to stand after being stirred evenly to obtain a geopolymer precursor; the geopolymer precursor is placed in a mold and vibrated to form, and cured at room temperature to a preset age.

[0023] In some embodiments,

[0024] In the preparation of the geopolymer precursor, the magnesium oxide and the metakaolin are mixed and stirred at a first stirring speed, and after the phosphate solution is added and allowed to stand, the mixture is stirred at a second stirring speed, wherein the second stirring speed is greater than the first stirring speed;

[0025] Specifically, the first stirring speed is 120-160±5r / min for rotation and 56-68±5r / min for revolution, and the second stirring speed is 275-295±10r / min for rotation and 115-135±10r / min for revolution;

[0026] More preferably, the first stirring speed is 140±5 r / min for rotation and 62±5 r / min for revolution, and the second stirring speed is 285±10 r / min for rotation and 125±10 r / min for revolution.

[0027] The present application provides a method for preparing a metakaolin-based phosphate geopolymer, comprising: using metakaolin and a phosphate solution as raw materials, adding magnesium oxide, and stirring evenly; and curing at room temperature until a preset age.

[0028] This application has the following beneficial effects:

[0029] By using kaolin and phosphate solution as reaction raw materials and adding magnesium oxide additives, the synthesis and curing of geopolymers can be achieved at room temperature. No temperature increase operation is required, the process is simple, a large amount of energy can be saved, and it is easy to apply in engineering.

[0030] At the same time, the raw materials used are rich, and no heating operation is required. The geopolymer does not need to be heated and solidified, and can be solidified at room temperature by itself, which has the advantages of low energy consumption, simple process, and low production cost. In addition, the entire preparation process does not produce any toxic pollutants, which is safe and environmentally friendly. The prepared metakaolin-based phosphate geopolymer has good mechanical properties and a short room temperature curing and condensation time, which is conducive to the application of practical engineering. DETAILED DESCRIPTION

[0031] The following will be combined with the specific embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present application and its application or use. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0032] In addition, it should be noted that the use of terms such as "first" and "second" to limit is only for the convenience of distinguishing the same features. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of this application.

[0033] A method for preparing a metakaolin-based phosphate geopolymer comprises:

[0034] Take metakaolin and phosphate solution as raw materials, add magnesium oxide, stir evenly; let stand and cure at room temperature until the preset age.

[0035] The kaolin-based phosphate geopolymer mainly uses kaolin and phosphoric acid or phosphate as the reaction raw materials. Its reaction mechanism is similar to that of alkali-activated geopolymer, which is mainly divided into three stages: depolymerization, polycondensation, and gel networking. 2 With Al 2 O 3 It depolymerizes under the action of phosphate solution and is free in the solution as a monomer. In an acid environment, the covalent bond with the oxygen atom is broken to form orthoaluminosilicate. The phosphate ion enters the Al-O to balance the Al 3+ The negative charge of MgO is formed by polymerization to form a three-dimensional network structure. Magnesium oxide has a higher solubility under acidic conditions and takes precedence over SiO 2 With Al 2 O 3 Dissolving under acidic conditions, the dissolved magnesium ions combine with phosphate ions to generate phosphate inorganic gelling materials that are beneficial to the development of matrix material performance.

[0036] In the following examples, the kaolin-based phosphate geopolymer prepared under room temperature conditions proposed in the present application can significantly reduce its setting time under room temperature conditions without significantly affecting its strength, compared with the blank control group without adding admixtures, thereby reducing time costs and facilitating its application in practical engineering.

[0037] Example 1

[0038] A method for preparing a metakaolin-based phosphate geopolymer under room temperature conditions, comprising mixing a phosphoric acid solution and aluminum hydroxide at a P / Al molar ratio of 3.0, slowly adding a certain amount of distilled water while stirring, preparing a phosphate solution with a mass fraction of 58%, and aging the mixture at room temperature for 24 hours after stirring. The magnesium oxide and the metakaolin are mixed and stirred at a first stirring speed (rotation 140±5r / min, revolution 62±5r / min), and after the phosphate solution is added and allowed to stand, the mixture is stirred at a second stirring speed (rotation 285±10r / min, revolution 125±10r / min).

[0039] Subsequently, the total mass of solid (metakaolin + magnesium oxide) was mixed with a phosphate solution in a mass ratio of 0.66 (solid to activator P:Al = 0.36:1.01 (molar ratio), where Al is only calculated in the solid metakaolin), and 0% magnesium oxide was added as a blank control group, and the mixture was stirred, poured into a mold and vibrated to form.

[0040] Referring to the "Test Methods for Water Consumption, Setting Time and Stability of Cement Standard Consistency" GB / T1346, the initial setting time and final setting time of kaolin-based phosphate geopolymer cementitious materials were measured at room temperature to be 2104min and 3129min respectively; referring to the "Test Method for Strength of Cement Mortar" (GB / T 17671-2021), the flexural strength of kaolin-based phosphate geopolymer mortar at 7 days old was 5.537MPa, and the compressive strength was 52.1MPa; the flexural strength at 28 days old was 9.417MPa, and the compressive strength was 64.6MPa.

[0041] Example 2

[0042] A method for preparing a metakaolin-based phosphate geopolymer under room temperature conditions, comprising mixing a phosphoric acid solution and aluminum hydroxide at a P / Al molar ratio of 3.0, slowly adding a certain amount of distilled water while stirring, preparing a phosphate solution with a mass fraction of 58%, and aging the mixture at room temperature for 24 hours after stirring. The magnesium oxide and the metakaolin are mixed and stirred at a first stirring speed (rotation 140±5r / min, revolution 62±5r / min), and after the phosphate solution is added and allowed to stand, the mixture is stirred at a second stirring speed (rotation 285±10r / min, revolution 125±10r / min).

[0043] Subsequently, the total mass of solid (metakaolin + magnesium oxide) was mixed with a phosphate solution in a mass ratio of 0.66 (solid to activator P:Al:Mg=0.37:1.01:0.0375 (molar ratio), wherein Al is only calculated in the solid metakaolin), 1.5% magnesium oxide was added, and the mixture was stirred, poured into a mold and vibrated to form.

[0044] Referring to the "Test Methods for Water Consumption, Setting Time and Stability of Cement Standard Consistency" GB / T1346, the initial setting time and final setting time of kaolin-based phosphate geopolymer cementitious materials were measured at room temperature to be 1360min and 1720min respectively; referring to the "Test Method for Strength of Cement Mortar" (GB / T 17671-2021), the flexural strength of kaolin-based phosphate geopolymer mortar at 7 days old was 6.978MPa, and the compressive strength was 56.0MPa; the flexural strength at 28 days old was 9.103MPa, and the compressive strength was 52.7MPa.

[0045] Example 3

[0046] A method for preparing a metakaolin-based phosphate geopolymer under room temperature conditions, comprising mixing a phosphoric acid solution and aluminum hydroxide at a P / Al molar ratio of 3.0, slowly adding a certain amount of distilled water while stirring, preparing a phosphate solution with a mass fraction of 58%, and aging the mixture at room temperature for 24 hours after stirring. The magnesium oxide and the metakaolin are mixed and stirred at a first stirring speed (rotation 140±5r / min, revolution 62±5r / min), and after the phosphate solution is added and allowed to stand, the mixture is stirred at a second stirring speed (rotation 285±10r / min, revolution 125±10r / min).

[0047] Subsequently, the total mass of solid (metakaolin + magnesium oxide) was mixed with phosphate solution in a mass ratio of 0.66 (solid and activator P:Al:Mg = 0.37:1.01:0.075 (molar ratio), where Al is only calculated in solid metakaolin), 3% magnesium oxide was added, and the mixture was stirred, poured into a mold and vibrated to form.

[0048] Referring to the "Test Method for Water Consumption, Setting Time and Stability of Cement Standard Consistency" GB / T1346, the initial setting time and final setting time of kaolin-based phosphate geopolymer cementitious materials were measured at room temperature to be 1066min and 1277min respectively; referring to the "Test Method for Strength of Cement Mortar" (GB / T 17671-2021), the flexural strength of kaolin-based phosphate geopolymer mortar at 7 days old was 8.653MPa, and the compressive strength was 46.8MPa; the flexural strength at 28 days old was 11.342MPa, and the compressive strength was 65.6MPa.

[0049] Example 4

[0050] A method for preparing a metakaolin-based phosphate geopolymer under room temperature conditions comprises mixing a phosphoric acid solution and aluminum hydroxide at a P / Al molar ratio of 2.0, slowly adding a certain amount of distilled water while stirring, preparing a phosphate solution with a mass fraction of 58%, and aging the mixture at room temperature for 24 hours after stirring. The magnesium oxide and the metakaolin are mixed and stirred at a first stirring speed (rotation 140±5r / min, revolution 62±5r / min), and after the phosphate solution is added and allowed to stand, the mixture is stirred at a second stirring speed (rotation 285±10r / min, revolution 125±10r / min).

[0051] Subsequently, the total mass of solid (metakaolin + magnesium oxide) was mixed with a phosphate solution in a mass ratio of 0.66 (solid to activator P:Al = 0.36:1.01 (molar ratio), where Al is only calculated in the solid metakaolin), and 0% magnesium oxide was added as a blank control group, and the mixture was stirred, poured into a mold and vibrated to form.

[0052] Referring to the "Test Method for Strength of Cement Mortar" (GB / T 17671-2021), the flexural strength of kaolin-based phosphate geopolymer mortar at 7 days old was 3.530 MPa, and the compressive strength was 32.1 MPa; the flexural strength at 28 days old was 4.836 MPa, and the compressive strength was 47.0 MPa.

[0053] Example 5

[0054] A method for preparing a metakaolin-based phosphate geopolymer under room temperature conditions, comprising mixing a phosphoric acid solution and aluminum hydroxide at a P / Al molar ratio of 4.0, slowly adding a certain amount of distilled water while stirring, preparing a phosphate solution with a mass fraction of 58%, and aging the mixture at room temperature for 24 hours after stirring. The magnesium oxide and the metakaolin are mixed and stirred at a first stirring speed (rotation 140±5r / min, revolution 62±5r / min), and after the phosphate solution is added and allowed to stand, the mixture is stirred at a second stirring speed (rotation 285±10r / min, revolution 125±10r / min).

[0055] Subsequently, the total mass of solid (metakaolin + magnesium oxide) was mixed with a phosphate solution in a mass ratio of 0.66 (solid to activator P:Al = 0.36:1.01 (molar ratio), where Al is only calculated in the solid metakaolin), and 0% magnesium oxide was added as a blank control group, and the mixture was stirred, poured into a mold and vibrated to form.

[0056] Referring to the "Test Method for Strength of Cement Mortar" (GB / T 17671-2021), the flexural strength of kaolin-based phosphate geopolymer mortar at 7 days old was 3.000 MPa, and the compressive strength was 30.5 MPa; the flexural strength at 28 days old was 5.322 MPa, and the compressive strength was 53.5 MPa.

[0057] By comparing the 7d and 28d flexural and compressive strengths when the molar ratio of phosphoric acid to the aluminum hydroxide in the phosphoric acid solution is 2:1, 3:1, and 4:1, respectively, the optimal molar ratio of phosphoric acid to the aluminum hydroxide in the phosphoric acid solution is 3:1.

[0058] Through the above examples, it can be seen that the use of magnesium oxide as an admixture added to the preparation of metakaolin-based phosphate geopolymer can improve the flexural strength and compressive strength of the geopolymer. The addition of magnesium oxide provides a magnesium source that preferentially reacts with phosphate for the polymerization reaction, and has a greater affinity than the blank group. Without excessive loss of strength, it not only increases the polymerization reaction speed, but also effectively shortens the curing time, allowing it to be quickly formed at room temperature.

[0059] It is easy for those skilled in the art to understand that the above-mentioned implementation modes can be freely combined and superimposed without conflict.

[0060] The above is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements and improvements made within the spirit and principles of the present application shall be included in the protection scope of the present application. The above is only a preferred implementation of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present application, and these improvements and variations should also be regarded as the protection scope of the present application.

Claims

1. A method for preparing a metakaolin-based phosphate geopolymer, characterized in that: include: Take metakaolin and phosphate solution as raw materials, add magnesium oxide, and stir evenly; Allow to cure at room temperature until the preset age.

2. The preparation method according to claim 1, characterized in that: Also includes: The phosphate solution is prepared by mixing a phosphoric acid solution with aluminum hydroxide and aging for a preset period of time.

3. The preparation method according to claim 2, characterized in that: The molar ratio of phosphoric acid to aluminum hydroxide in the phosphoric acid solution is set to 2-4:

1.

4. The preparation method according to claim 3, characterized in that: The mass percentage concentration of the phosphoric acid solution is set to 75-85%, and the mass percentage concentration of the prepared phosphate solution is 50-60%.

5. The preparation method according to any one of claims 2 to 4, characterized in that: The preset time period is set to 18-30 hours.

6. The preparation method according to any one of claims 2 to 4, characterized in that: The percentage of magnesium oxide to the mass of the metakaolin is set to m, and satisfies 0% <m≤3%。 7. The preparation method according to claim 6, characterized in that: The molar ratio of the metakaolin to the phosphate solution is set to Al:P=0.36-0.40:1.01-1.

10.

8. The preparation method according to claim 7, characterized in that: The magnesium oxide and the metakaolin are mixed and stirred, the phosphate solution is added dropwise during the stirring process, and the mixture is allowed to stand after being stirred evenly to obtain a geopolymer precursor; the geopolymer precursor is placed in a mold and vibrated to form, and cured at room temperature to a preset age.

9. The preparation method according to claim 8, characterized in that: In the preparation of the geopolymer precursor, the magnesium oxide and the metakaolin are mixed and stirred at a first stirring speed, and after the phosphate solution is added and allowed to stand, the mixture is stirred at a second stirring speed, wherein the second stirring speed is greater than the first stirring speed; Specifically, the first stirring speed is 120-160±5 r / min for rotation and 56-68±5 r / min for revolution, and the second stirring speed is 275-295±10 r / min for rotation and 115-135±10 r / min for revolution; More preferably, the first stirring speed is 140±5 r / min for rotation and 62±5 r / min for revolution, and the second stirring speed is 285±10 r / min for rotation and 125±10 r / min for revolution.

10. A metakaolin-based phosphate geopolymer obtained by the preparation method according to any one of claims 1 to 9.