Concrete resistant to chloride ion permeation and construction method

By using modified materials and optimizing proportions in ready-mixed concrete, the anti-chlorine ion penetration performance is improved, the problem of insufficient durability of concrete in the existing technology is solved, and the quality of efficient production and construction is guaranteed, which is suitable for high-durance. sexual construction projects.

CN118955054APending Publication Date: 2024-11-15CCCC THIRD HARBOR ENGINEERING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411114419.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing ready-mixed concrete has insufficient durability, especially its poor resistance to chloride ion penetration, which affects the service life and safety of construction projects.

Method used

Using cement, fly ash, modified carbon fiber, modified composite silicon powder and modified polycarboxylic acid water reducer, the density of concrete and anti-chlorine ion penetration performance are improved through scientific proportion design and modification treatment. , combined with optimized construction methods, ensure efficient production and stable quality of concrete.

Benefits of technology

It significantly improves the compressive strength, flexural strength, permeability and chloride ion permeability of concrete, extends the service life of buildings, is suitable for construction projects with high durability requirements such as marine engineering and bridges, and ensures construction. quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993223640000081
    Figure BDA0004993223640000081
  • Figure BDA0004993223640000091
    Figure BDA0004993223640000091
Patent Text Reader

Abstract

The invention relates to the technical field of building engineering materials, in particular to chloride ion permeation resistant concrete and a construction method. The chloride ion permeation resistant concrete is prepared from the following preparation raw materials in parts by mass: 200 to 250 parts of cement, 60 to 80 parts of fly ash, 1000 to 1200 parts of sandstone, 12 to 15 parts of modified carbon fiber, 15 to 20 parts of modified composite silicon powder, 7 to 10 parts of modified polycarboxylic acid water reducing agent, 2 to 3 parts of accelerant and 120 to 150 parts of water. According to the chloride ion permeation resistant concrete disclosed by the invention, high compactness, excellent compressive strength and breaking strength and excellent chloride ion permeation resistance are realized through careful material selection and scientific proportioning design. The performance is improved, so that the service life and durability of the concrete in a severe environment are remarkably enhanced, and the concrete is particularly suitable for constructional engineering such as ocean engineering, bridges and expressways with high durability requirements. In addition, by means of the construction method, the quality stability of the concrete is guaranteed, and the requirement for efficient production can be met while the construction quality is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of building engineering materials, and in particular to a concrete resistant to chloride ion penetration and a construction method. Background Art

[0002] At present, the raw materials of ready-mixed concrete come from different sources, with different technical levels and control methods. The technical indicators and performance of concrete produced by most ready-mixed concrete companies still remain at the level of traditional concrete, that is, the working performance and strength of concrete are the main control indicators. In terms of durability, most of them only consider the single indicator of anti-(water) permeability grade. The durability of concrete directly affects the service life of construction projects and is closely related to human life safety. With the development and growth of the ready-mixed concrete industry, concrete with good durability is more and more widely used in construction projects, and people's understanding of the durability of concrete is also deepening. As the key direction of concrete research, the comprehensive durability of ready-mixed concrete is also increasingly valued, and people's performance requirements for ready-mixed concrete are also getting higher and higher.

[0003] The chloride ion penetration resistance of concrete is one of the most important indicators for measuring the durability of concrete. The chloride ion penetration resistance of concrete is a comprehensive indicator of the concrete's resistance to water, oil and chloride ion penetration. It is used to evaluate the concrete's ability to resist the penetration of water, ions and other media, and reflects the density and overall durability of the concrete. The chloride ion penetration resistance of ready-mixed concrete is a very important aspect of the durability research of ready-mixed concrete. It can improve the comprehensive durability of concrete from the source and ensure quality. Summary of the invention

[0004] The purpose of this application is to provide a chloride ion penetration resistant concrete and construction method to address the deficiencies of current technologies, improve the comprehensive durability of concrete, and ensure construction quality. The chloride ion penetration resistant concrete prepared in this application has good compressive strength, flexural strength, impermeability grade and excellent chloride ion penetration resistance.

[0005] In a first aspect, the present application provides a concrete resistant to chloride ion penetration, which adopts the following technical solution: A concrete resistant to chloride ion penetration comprises the following raw materials, measured by weight: 200-250 parts of cement, 60-80 parts of fly ash, 1000-1200 parts of sand and gravel, 12-15 parts of modified carbon fiber, 15-20 parts of modified composite silicon powder, 7-10 parts of modified polycarboxylic acid water reducer, 2-3 parts of accelerator and 120-150 parts of water.

[0006] By adopting the above technical solutions, cement: as a basic bonding material, provides the basic strength and structural framework of concrete. Fly ash: as an auxiliary cementitious material, the addition of fly ash not only improves the later strength of concrete by its own volcanic ash activity, but also improves the compactness of concrete due to its fine particle filling effect, thereby enhancing the resistance to chloride ion penetration. Sand and gravel: constitute the skeleton of concrete, providing volume stability and mechanical strength. Modified carbon fiber: through surface modification, the bonding force between carbon fiber and cement matrix is ​​improved, the tensile strength and flexural strength of concrete are increased, and at the same time, the addition of carbon fiber also helps to disperse stress and reduce the generation of cracks, thereby indirectly improving the resistance to chloride ion penetration. Modified composite silica powder: after special modification, the surface strength of silica powder is improved, the water demand is reduced, and the ion adsorption capacity is enhanced. Modified silica powder fills the gaps between cement materials, further enhancing the compactness of concrete, and plays a key role in improving the resistance to chloride ion penetration. Modified polycarboxylate water reducer: With special structure and performance, it can effectively reduce the amount of concrete mixing water, reduce the porosity of cement, improve the density of concrete, and thus enhance its resistance to chloride ion penetration. Accelerator: Accelerate the early strength development of concrete and improve crack resistance, thereby enhancing the comprehensive durability and resistance to chloride ion penetration of concrete. Water: As a reaction medium and construction regulator, it ensures the correct proportion and workability of concrete. Modified carbon fiber and modified composite silica fume: Carbon fiber provides a reinforced skeleton and crack control, while modified silica fume improves the mechanical strength and impermeability of concrete by filling and enhancing interface interactions. Modified polycarboxylate water reducer and modified composite silica fume: Both improve the density of concrete. The water reducer reduces the water demand, and the silica fume reduces the penetration channel of chloride ions by physically filling and enhancing the ion adsorption capacity. Accelerator and cement: The accelerator accelerates the hydration process of cement, improves the early strength of concrete, and combines with the basic bonding properties of cement to jointly improve the overall performance of concrete. The chloride ion penetration-resistant concrete of the present application has achieved high density, excellent compressive strength and flexural strength, and excellent resistance to chloride ion penetration through careful material selection and scientific mix design. The improvement of these properties significantly enhances the service life and durability of concrete in harsh environments, and is particularly suitable for construction projects with high durability requirements such as marine engineering, bridges, and highways. In addition, the construction method of the present application ensures the quality stability of the concrete, so that it can meet the needs of efficient production while ensuring the construction quality.

[0007] Preferably, the method for preparing the modified composite silicon powder comprises the following steps: S21. Add 5 parts of D113 macroporous weakly acidic acrylic acid cation exchange resin to 100 parts of silicon powder according to the mass fraction, stir evenly for 30-40 minutes, then add the obtained mixture to 500 parts of 5% polyvinyl alcohol aqueous solution, stir for 150 minutes, remove the silicon powder by filtering, dry at 160° C. for 50-60 minutes, and cool to obtain modified silicon powder; S22. Dissolve 30 parts of butyl titanate in 50 parts of anhydrous ethanol solvent according to the mass fraction, and vigorously stir at a speed of 3000 r / min for 30 minutes to obtain a titanium source solution; add 50 parts of anhydrous ethanol, 20 parts of silicic acid and 5 parts of distilled water into a beaker and vigorously stir for 20 minutes, then drop the titanium source solution therein at a speed of 600 r / min, and stir the reaction at 35°C for 12 hours to obtain a nano titanium dioxide sol; S23. Add 30 parts of modified silicon powder to 100 parts of nano-titanium dioxide sol according to the mass fraction, stir for 30 minutes, ultrasonically disperse for 30-40 minutes, continue stirring for 3 hours, vacuum filter, and dry in a vacuum drying oven at 110°C for 8 hours to obtain modified composite silicon powder.

[0008] By adopting the above technical scheme, in the preparation of concrete resistant to chloride ion penetration, the preparation method of modified composite silica powder involves the following steps: silica powder is mixed and modified with cation exchange resin (S21): First, D113 macroporous weakly acidic acrylic cation exchange resin is uniformly stirred with silica powder. This process utilizes the macroporous characteristics and strong adhesion of the ion exchange resin to enhance the surface strength of silica powder particles and reduce the water demand. Then, the mixture is added to a polyvinyl alcohol aqueous solution and continued to be stirred, and then filtered and dried to obtain modified silica powder. This step improves the ion adsorption capacity of silica powder and increases the density of concrete by filling the gaps between cement materials. Preparation and application of nano titanium dioxide sol (S22): Nano titanium dioxide sol is prepared by dissolving butyl titanate in anhydrous ethanol and reacting it with an ethanol aqueous solution containing silica under vigorous stirring. This sol can further improve the dispersibility of particles in the process of modifying silica powder, while improving the surface strength of silica powder particles. Composite modification of silica powder and nano-titanium dioxide sol (S23): The modified silica powder is added to the nano-titanium dioxide sol, and after stirring and ultrasonic dispersion, the silica powder particles are evenly coated by the nano-titanium dioxide sol, and then vacuum filtered and dried to obtain the final modified composite silica powder. This step deepens the surface modification effect of silica powder, making it have better dispersibility and stronger interface interaction in concrete. The modified composite silica powder fills the gaps between cement materials, enhances the density of concrete, reduces the penetration channels of chloride ions, and works together with cement to improve the compressive strength and impermeability of concrete. While the modified composite silica powder improves the density of concrete, the modified polycarboxylic acid water reducer further increases the density of concrete by reducing the water demand. The two together significantly improve the resistance to chloride ion penetration. The modified carbon fiber enhances the tensile strength and flexural strength of concrete, while the modified composite silica powder enhances the durability and crack resistance of concrete by enhancing the density and ion adsorption capacity.

[0009] Preferably, the fly ash is Class I fly ash, and the 45 μm sieve residue of the fly ash is 23%.

[0010] Preferably, the sand and gravel have a particle size range of 0.1-1 mm and a SiO2 content greater than 95%.

[0011] Preferably, the cement is ordinary Portland cement of grade P·O42.5.

[0012] Preferably, the preparation method of the modified carbon fiber is as follows: according to the mass fraction, 100 parts of carbon fiber with a length of 2-5 mm and 200 parts of pure water are mixed evenly, the temperature is raised to 33°C, ozone is introduced into the solution at a rate of 4L / min for 40 minutes, and then the ozone supply is stopped; the solution is sealed, heated to 60°C, and allowed to stand for 4 hours; the solution is stirred for 30 minutes in an open state, 20 parts of 3-aminopropyltriethoxysilane ethanol solution with a mass concentration of 5% are added, heated to 43°C and stirred for 50 minutes, and then 10 parts of nano-titanium dioxide with a particle size of 50 nanometers are added, stirred for 30 minutes, the nano-titanium dioxide is coated on the surface of the carbon fiber, filtered, rinsed with water 3 times, and vacuum dried at 80°C to obtain modified carbon fiber.

[0013] By adopting the above technical scheme, the preparation method of modified carbon fiber involves the following key steps: Ozone treatment: First, the carbon fiber is mixed with pure water and ozone is introduced at a specific temperature. This process aims to activate the surface of the carbon fiber through the strong oxidizing effect of ozone, increase the oxygen-containing functional groups on its surface, such as carboxyl, hydroxyl, etc., which can enhance the chemical bonding between the carbon fiber and organic materials such as resin. Heating and standing: After ozone treatment, the solution is sealed and heated to a higher temperature for standing. The purpose of this step is to use the residual heat to promote the reorganization and stabilization of the functional groups on the surface of the carbon fiber, making it easier to react with the subsequent modifier. Surface modification: Under stirring conditions, 3-aminopropyl triethoxysilane ethanol solution is added to the solution, and stirring is continued at a specific temperature, and then nano titanium dioxide is added. As a coupling agent, the amino group in the molecule of 3-aminopropyl triethoxysilane can react with the oxygen-containing functional groups on the surface of the carbon fiber, and its ethoxy group can react with the hydroxyl group on the surface of the nano titanium dioxide, thereby forming a uniform nano titanium dioxide coating on the surface of the carbon fiber. The addition of nano-titanium dioxide not only enhances the surface strength of carbon fiber, but also improves its UV resistance and chemical corrosion resistance. Filtration, rinsing and drying: Finally, after filtration, water rinsing and vacuum drying, the final modified carbon fiber is obtained. The modified carbon fiber significantly improves the tensile strength and flexural strength of concrete by improving the bonding force between the cement matrix and effectively transferring and dispersing stress. In addition, the addition of carbon fiber can also improve the crack resistance of concrete, thereby indirectly improving the resistance to chloride ion penetration. The modified carbon fiber enhances the mechanical properties of concrete, while the modified composite silica fume further increases the density of concrete through the filling effect and the improvement of ion adsorption capacity. The two work together to improve the resistance of concrete to chloride ion penetration from a physical and chemical perspective. The modified carbon fiber provides good mechanical properties, while the modified polycarboxylate water reducer reduces the penetration channel of chloride ions by reducing the water demand and improving the density of concrete, and enhances the durability and resistance to chloride ion penetration of concrete. In summary, the introduction of modified carbon fiber not only improves the mechanical strength and crack resistance of concrete, but also significantly improves the concrete's resistance to chloride ion penetration through the synergistic effect with modified composite silica fume and modified polycarboxylic acid water reducer.

[0014] Preferably, the preparation method of the modified polycarboxylate water-reducing agent comprises the following steps: S71, add 18 mol of acrylic acid and 1 mol of methyltrimethoxysilane to 6 kg of water, stir evenly, and obtain a mixed solution A; S72, add 0.4 mol of vitamin C and 0.9 mol of 3-mercaptopropionic acid to 3 kg of water, stir evenly, and obtain a mixed solution B; S73. Add 1 mol of benzoic anhydride modified methyl allyl polyoxyethylene ether and 7 mol of isopentanol polyoxyethylene ether to 25 kg of water and stir, then add 1 mol of hydrogen peroxide, stir and heat to 48°C, then drop mixed solution A and mixed solution B at the same time. After the addition is completed for 4 hours, continue stirring and reacting for 4 hours, then add NaOH aqueous solution to adjust the pH value to 7, and obtain a modified polycarboxylic acid water reducer.

[0015] By adopting the above technical scheme, the preparation method of the modified polycarboxylic acid water-reducing agent involves multiple chemical reaction steps, which work together to generate a water-reducing agent with special structure and performance, thereby improving the density of concrete. The improvement in density can effectively prevent the corrosion of chloride ions, thereby enhancing the concrete's resistance to chloride ion penetration and durability.

[0016] Preferably, the accelerator comprises the following raw materials, calculated by weight: 100 parts of hydroxyethyl acrylate, 0.2 parts of dicumyl peroxide, 8.5 parts of bis(allyl alcohol)-terminated polyoxyethylene ether, 5 parts of triisopropanolamine, 6.3 parts of 1-amino-2-methyl-2-propanol, 130 parts of acetone, and 90 parts of water.

[0017] Preferably, the preparation method of the accelerator is: according to the mass parts, hydroxyethyl acrylate, diisopropylbenzene peroxide, bis(allyl alcohol)-terminated polyoxyethylene ether, triisopropanolamine, 1-amino-2-methyl-2-propanol, acetone and water are stirred for 30-40 minutes to obtain the accelerator.

[0018] Preferably, the preparation method of the accelerator is: according to the mass parts, hydroxyethyl acrylate, diisopropylbenzene peroxide, bis(allyl alcohol)-terminated polyoxyethylene ether, triisopropanolamine, 1-amino-2-methyl-2-propanol, acetone and water are stirred for 40-50 minutes to obtain the accelerator.

[0019] In a second aspect, the present application provides a construction method for chloride ion penetration-resistant concrete, which adopts the following technical solution: As a general technical concept, the present application also provides a construction method for the above-mentioned chloride ion penetration-resistant concrete, comprising the following steps: S101. First, cement, fly ash, sand and gravel, modified carbon fiber, modified composite silica powder, modified polycarboxylic acid water reducer, accelerator and water are uniformly mixed according to the mass fractions to obtain concrete; S102. Pour the concrete in layers, vibrate each layer to make it dense, cover the concrete tightly with plastic film after it is smoothed, and carry out moisture-proof maintenance on the concrete surface after the concrete is finally set; wherein, the slump of the concrete into the mold is 160-190mm, the temperature into the mold is ≤38℃, the layer thickness is ≤45cm, and the maintenance time is ≥7 days.

[0020] In summary, the beneficial technical effects of this application are: 1. Improved resistance to chloride ion penetration: By using modified composite silica fume and modified polycarboxylate water reducer, the density of concrete is significantly improved, thus effectively preventing chloride ion erosion. This feature is particularly important for buildings in coastal or salty environments, as these environments usually accelerate the corrosion process of steel bars in concrete.

[0021] 2. Enhanced mechanical properties: The addition of modified carbon fiber enhances the interface strength between it and other components of the mortar through surface modification technology, thereby improving the compressive and flexural strength of the concrete. This means that the concrete structure can not only withstand greater loads, but also better resist impact and deformation.

[0022] 3. Improved overall durability: The durability of concrete has been comprehensively improved, including better impermeability and durability, as well as improved crack resistance. These characteristics ensure that the concrete structure can maintain its performance and appearance during long-term application, reducing the need for maintenance and repair.

[0023] 4. Economic benefits: Without sacrificing performance, by using fly ash as a partial substitute material, the amount of cement used is reduced, thereby reducing costs. At the same time, the use of modified composite silica fume not only reduces the cost of silica fume, but also improves the overall performance of concrete.

[0024] 5. Environmentally friendly: The concrete formula of this application takes environmental factors into consideration, and by reducing chloride ion erosion, it prolongs the service life of the building and reduces the generation of construction waste. In addition, the modified materials and accelerators used are all designed to reduce the negative impact on the environment.

[0025] 6. Guarantee of construction quality: Due to the excellent performance of concrete, the quality of the construction process is guaranteed, reducing the rework and repair work caused by quality problems, speeding up the construction progress and improving construction efficiency. DETAILED DESCRIPTION

[0026] The implementation scheme of the present application will be described in detail below in conjunction with the examples, but those skilled in the art will understand that the following examples are only used to illustrate the present application and should not be considered to limit the scope of the present application. If the specific conditions are not specified in the examples, they are carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially. The fly ash is Class I fly ash, and the 45μm sieve residue of the fly ash is 23%. The particle size range of sand and gravel is 0.1-1mm, the SiO2 content is greater than 95%, and the cement is P·O42.5 grade ordinary Portland cement.

[0027] In the following examples and preparation examples, 1 part means 1 kg.

[0028] Preparation Example 1 Preparation of modified composite silicon powder The preparation method of modified composite silicon powder comprises the following steps: S21, according to the mass fraction, add 5 parts of D113 macroporous weakly acidic acrylic acid cation exchange resin to 100 parts of silicon powder, stir evenly for 35 minutes, then add the obtained mixture to 500 parts of 5% polyvinyl alcohol aqueous solution, stir for 150 minutes, remove the silicon powder by filtration, dry at 160°C for 55 minutes, and cool to obtain modified silicon powder; S22. Dissolve 30 parts of butyl titanate in 50 parts of anhydrous ethanol solvent according to the mass fraction, and vigorously stir at a speed of 3000 r / min for 30 minutes to obtain a titanium source solution; add 50 parts of anhydrous ethanol, 20 parts of silicic acid and 5 parts of distilled water into a beaker and vigorously stir for 20 minutes, then drop the titanium source solution therein at a speed of 600 r / min, and stir the reaction at 35°C for 12 hours to obtain a nano titanium dioxide sol; S23. Add 30 parts of modified silicon powder to 100 parts of nano-titanium dioxide sol according to the mass fraction, stir for 30 minutes, ultrasonically disperse for 35 minutes, continue stirring for 3 hours, vacuum filter, and dry in a vacuum drying oven at 110°C for 8 hours to obtain modified composite silicon powder.

[0029] Preparation Example 2 Preparation of modified carbon fiber The preparation method of the modified carbon fiber is as follows: according to the mass fraction, 100 parts of carbon fiber with a length of 2-5 mm and 200 parts of pure water are mixed evenly, the temperature is raised to 33° C., ozone is introduced into the solution at a speed of 4 L / min for 40 minutes, and then the ozone supply is stopped; the solution is sealed, heated to 60° C., and allowed to stand for 4 hours; the solution is stirred for 30 minutes in an open state, 20 parts of 3-aminopropyltriethoxysilane ethanol solution with a mass concentration of 5% are added, heated to 43° C. and stirred for 50 minutes, and then 10 parts of nano-titanium dioxide with a particle size of 50 nanometers are added, stirred for 30 minutes, the nano-titanium dioxide is coated on the surface of the carbon fiber, filtered, rinsed with water 3 times, and vacuum dried at 80° C. to obtain the modified carbon fiber.

[0030] Preparation Example 3 Preparation of modified polycarboxylate water reducer The preparation method of the modified polycarboxylate water-reducing agent comprises the following steps: S71, add 18 mol of acrylic acid and 1 mol of methyltrimethoxysilane to 6 kg of water, stir evenly, and obtain a mixed solution A; S72, add 0.4 mol of vitamin C and 0.9 mol of 3-mercaptopropionic acid to 3 kg of water, stir evenly, and obtain a mixed solution B; S73. Add 1 mol of benzoic anhydride modified methyl allyl polyoxyethylene ether and 7 mol of isopentanol polyoxyethylene ether to 25 kg of water and stir, then add 1 mol of hydrogen peroxide, stir and heat to 48°C, then drop mixed solution A and mixed solution B at the same time. After the addition is completed for 4 hours, continue stirring and reacting for 4 hours, then add NaOH aqueous solution to adjust the pH value to 7, and obtain a modified polycarboxylic acid water reducer.

[0031] Preparation Example 4 Preparation of accelerator The preparation method of the accelerator is as follows: according to the mass parts, 100 parts of hydroxyethyl acrylate, 0.2 parts of diisopropylbenzene peroxide, 8.5 parts of bis(allyl alcohol)-terminated polyoxyethylene ether, 5 parts of triisopropanolamine, 6.3 parts of 1-amino-2-methyl-2-propanol, 130 parts of acetone and 90 parts of water are stirred for 35 minutes to obtain the accelerator.

[0032] Example 1 A concrete resistant to chloride ion penetration comprises the following raw materials: 200 parts of cement, 60 parts of fly ash, 1000 parts of sand and gravel, 12 parts of modified carbon fiber, 15 parts of modified composite silicon powder, 7 parts of modified polycarboxylic acid water reducer, 2 parts of accelerator and 120 parts of water.

[0033] The above-mentioned construction method of concrete resistant to chloride ion penetration comprises the following steps: S101. First, cement, fly ash, sand and gravel, modified carbon fiber, modified composite silica powder, modified polycarboxylic acid water reducer, accelerator and water are uniformly mixed according to the mass fractions to obtain concrete; S102. Pour the concrete in layers, vibrate each layer to make it dense, cover the concrete tightly with plastic film after it is smoothed, and carry out moisture-proof maintenance on the concrete surface after the concrete is finally set; wherein, the slump of the concrete into the mold is 160mm, the temperature into the mold is 38°C, the layer thickness is 45cm, and the maintenance time is 7 days.

[0034] Example 2 A concrete resistant to chloride ion penetration comprises the following raw materials: 250 parts of cement, 80 parts of fly ash, 1200 parts of sand and gravel, 15 parts of modified carbon fiber, 20 parts of modified composite silicon powder, 10 parts of modified polycarboxylic acid water reducer, 3 parts of accelerator and 150 parts of water.

[0035] The above-mentioned construction method of concrete resistant to chloride ion penetration comprises the following steps: S101. First, cement, fly ash, sand and gravel, modified carbon fiber, modified composite silica powder, modified polycarboxylic acid water reducer, accelerator and water are uniformly mixed according to the mass fractions to obtain concrete; S102, pouring concrete in layers, vibrating each layer to make it dense, and after smoothing the concrete, covering it tightly with plastic film, and after the concrete is finally set, performing moisture-maintaining maintenance on the concrete surface; wherein, the slump of the concrete into the mold is 190 mm, the temperature into the mold is 35° C., the layer thickness is 40 cm, and the maintenance time is 14 days.

[0036] Example 3 A concrete resistant to chloride ion penetration comprises the following raw materials: 220 parts of cement, 70 parts of fly ash, 1100 parts of sand and gravel, 14 parts of modified carbon fiber, 18 parts of modified composite silicon powder, 8 parts of modified polycarboxylic acid water reducer, 2.5 parts of accelerator and 130 parts of water.

[0037] The above-mentioned construction method of concrete resistant to chloride ion penetration comprises the following steps: S101. First, cement, fly ash, sand and gravel, modified carbon fiber, modified composite silica powder, modified polycarboxylic acid water reducer, accelerator and water are uniformly mixed according to the mass fractions to obtain concrete; S102, pouring concrete in layers, vibrating each layer to make it dense, and after smoothing the concrete, covering it tightly with plastic film, and after the concrete is finally set, performing moisture-maintaining maintenance on the concrete surface; wherein, the slump of the concrete into the mold is 180 mm, the temperature into the mold is 33° C., the layer thickness is 38 cm, and the maintenance time is 28 days.

[0038] Comparative Example 1 The same as Example 3, except that an equal amount of unmodified silicon powder in Preparation Example 1 is used instead of the modified composite silicon powder.

[0039] Comparative Example 2 Same as Example 3, except that an equal amount of unmodified carbon fibers (length 3-5 mm) are used instead of modified carbon fibers.

[0040] Comparative Example 3 The same as Example 3, except that an equal amount of polyhydroxy acid-based high-efficiency water reducer produced by Wuhan Jiyesheng Chemical Co., Ltd. is used instead of the modified polycarboxylic acid water reducer.

[0041] Comparative Example 4 The same as Example 3, except that the amount of accelerator added is 0 parts.

[0042] Performance Testing The chloride ion penetration resistant concrete obtained in Examples 1 to 3 and Comparative Examples 1 to 4 was made into test specimens. The specimens were cubes with a side length of 100 mm. The surfaces were sealed with a polyethylene film and cured at room temperature for 24 hours before demolding. The specimens were moved to a standard curing box and cured for the corresponding 28 days. The following tests were performed. The test results are shown in Table 1.

[0043] The mechanical properties are tested according to the national standard GB / T17671-2021; Chloride ion diffusion coefficient: Tested in accordance with the "Non-steady-state migration test of chloride ion migration coefficient of concrete - Chloride ion diffusion coefficient rapid test NTBUILD492" in GB / T50082-2009 "Standard for test methods of long-term performance and durability of ordinary concrete"; 28d electric flux: tested in accordance with GB / T50082-2009 "Standard for test methods of long-term performance and durability of ordinary concrete"; Water-resistance grade: tested in accordance with GB / T50082-2009 "Standard for test methods for long-term performance and durability of ordinary concrete".

[0044] Table 1 Performance test Analyzing the data in Table 1, we can see that: 1) The chloride ion penetration-resistant concrete prepared in Examples 1 to 3 has good compressive strength, flexural strength, impermeability grade and excellent chloride ion penetration resistance, which can significantly improve the comprehensive durability of concrete and ensure the construction quality.

[0045] 2) The performance comparison analysis of the chloride ion penetration-resistant concrete prepared in combination with Example 3 and Comparative Example 1 shows that the modified composite silica powder prepared in this application fills the gaps between cement materials, enhances the compactness of concrete, reduces the penetration channels of chloride ions, and works together with cement to improve the compressive strength and impermeability of concrete. While the modified composite silica powder improves the compactness of concrete, the modified polycarboxylate water-reducing agent further increases the density of concrete by reducing the water demand, and the two together significantly improve the chloride ion penetration resistance. The modified carbon fiber enhances the tensile strength and flexural strength of concrete, while the modified composite silica powder enhances the durability of concrete by enhancing compactness and ion adsorption capacity.

[0046] 3) The comparative analysis of the performance of the chloride ion penetration resistant concrete obtained in Example 3 and Comparative Example 2 shows that the surface modification of the modified carbon fiber by 3-aminopropyltriethoxysilane and titanium dioxide enhances the interface strength between the carbon fiber and other components of the mortar. This enhanced interface interaction helps to improve the overall mechanical properties of the mortar, including compressive strength and flexural strength.

[0047] 4) The comparative analysis of the performance of the chloride ion penetration-resistant concrete prepared in Example 3 and Comparative Example 3 shows that the modified polycarboxylate water-reducing agent prepared in the present application has a special structure, which improves the compactness of the concrete, and the improvement of the compactness can effectively prevent the erosion of chloride ions, thereby enhancing the chloride ion penetration resistance and durability of the concrete.

[0048] 5) The comparative analysis of the performance of the chloride ion penetration-resistant concrete obtained in Example 3 and Comparative Example 4 shows that the accelerator prepared in the application utilizes the synergistic effect between its components, which not only improves the early strength of the concrete, but also improves its mechanical properties, durability and chloride ion penetration resistance.

[0049] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.

Claims

1. A concrete resistant to chloride ion penetration, characterized in that: The preparation raw materials include the following by mass: 200-250 parts of cement, 60-80 parts of fly ash, 1000-1200 parts of sand and gravel, 12-15 parts of modified carbon fiber, 15-20 parts of modified composite silicon powder, 7-10 parts of modified polycarboxylic acid water reducer, 2-3 parts of accelerator and 120-150 parts of water.

2. The concrete resistant to chloride ion penetration according to claim 1, characterized in that: The preparation method of the modified composite silicon powder comprises the following steps: S21. Add 5 parts of D113 macroporous weakly acidic acrylic acid cation exchange resin to 100 parts of silicon powder according to the mass fraction, stir evenly for 30-40 minutes, then add the obtained mixture to 500 parts of 5% polyvinyl alcohol aqueous solution, stir for 150 minutes, remove the silicon powder by filtration, dry at 160°C for 50-60 minutes, and cool to obtain modified silicon powder; S22. Dissolve 30 parts of butyl titanate in 50 parts of anhydrous ethanol solvent according to the mass fraction, and vigorously stir at a speed of 3000 r / min for 30 minutes to obtain a titanium source solution; add 50 parts of anhydrous ethanol, 20 parts of silicic acid and 5 parts of distilled water into a beaker and vigorously stir for 20 minutes, then drop the titanium source solution therein at a speed of 600 r / min, and stir the reaction at 35°C for 12 hours to obtain a nano titanium dioxide sol; S23. Add 30 parts of modified silicon powder to 100 parts of nano-titanium dioxide sol according to the mass fraction, stir for 30 minutes, ultrasonically disperse for 30-40 minutes, continue stirring for 3 hours, vacuum filter, and dry in a vacuum drying oven at 110°C for 8 hours to obtain modified composite silicon powder.

3. The concrete resistant to chloride ion penetration according to claim 1, characterized in that: The fly ash is Class I fly ash, and the 45 μm sieve residue of the fly ash is 23%.

4. The concrete resistant to chloride ion penetration according to claim 1, characterized in that: The particle size of the sand and gravel is in the range of 0.1-1 mm, and the SiO2 content is greater than 95%.

5. The concrete resistant to chloride ion penetration according to claim 1, characterized in that: The cement is ordinary Portland cement of grade P·O42.

5.

6. The concrete resistant to chloride ion penetration according to claim 1, characterized in that: The modified carbon fiber preparation method comprises: mixing 100 parts of carbon fiber with a length of 2-5 mm and 200 parts of pure water in proportion by mass, heating the mixture to 33° C., introducing ozone into the solution at a rate of 4 L / min for 40 minutes, and then stopping the ozone supply; The solution was sealed, heated to 60°C, and allowed to stand for 4 hours; the solution was stirred for 30 minutes in an open state, 20 parts of 5% mass concentration of 3-aminopropyltriethoxysilane ethanol solution were added, heated to 43°C and stirred for 50 minutes, and then 10 parts of nano-titanium dioxide with a particle size of 50 nanometers were added and stirred for 30 minutes. The nano-titanium dioxide was coated on the surface of the carbon fiber, filtered, rinsed with water 3 times, and vacuum dried at 80°C to obtain modified carbon fiber.

7. The concrete resistant to chloride ion penetration according to claim 1, characterized in that: The preparation method of the modified polycarboxylate water-reducing agent comprises the following steps: S71, adding 18 mol of acrylic acid and 1 mol of methyltrimethoxysilane to 6 kg of water, stirring evenly, to obtain a mixed solution A; S72, add 0.4 mol vitamin C and 0.9 mol 3-mercaptopropionic acid to 3 kg water, stir evenly, and obtain a mixed solution B; S73. Add 1 mol of benzoic anhydride modified methyl allyl polyoxyethylene ether and 7 mol of isopentanol polyoxyethylene ether to 25 kg of water and stir, then add 1 mol of hydrogen peroxide, stir and heat to 48°C, then drop mixed solution A and mixed solution B at the same time. After the addition is completed for 4 hours, continue stirring and reacting for 4 hours, then add NaOH aqueous solution to adjust the pH value to 7, and obtain a modified polycarboxylic acid water reducer.

8. The concrete resistant to chloride ion penetration according to claim 1, characterized in that: The accelerator includes the following raw materials, calculated by weight: 100 parts of hydroxyethyl acrylate, 0.2 parts of dicumyl peroxide, 8.5 parts of bis(allyl alcohol)-terminated polyoxyethylene ether, 5 parts of triisopropanolamine, 6.3 parts of 1-amino-2-methyl-2-propanol, 130 parts of acetone, and 90 parts of water.

9. The concrete resistant to chloride ion penetration according to claim 8, characterized in that: The preparation method of the accelerator is as follows: according to the mass fractions, hydroxyethyl acrylate, diisopropylbenzene peroxide, bis(allyl alcohol)-terminated polyoxyethylene ether, triisopropanolamine, 1-amino-2-methyl-2-propanol, acetone and water are stirred for 40-50 minutes to obtain the accelerator.

10. A construction method for the chloride ion penetration resistant concrete according to any one of claims 1 to 9, characterized in that: The following steps are involved: S101. First, cement, fly ash, sand and gravel, modified carbon fiber, modified composite silica powder, modified polycarboxylic acid water reducer, accelerator and water are uniformly mixed according to the mass fractions to obtain concrete; S102. Pour the concrete in layers, vibrate each layer to make it dense, cover the concrete tightly with plastic film after it is smoothed, and carry out moisture-proof maintenance on the concrete surface after the concrete is finally set; wherein, the slump of the concrete into the mold is 160-190mm, the temperature into the mold is ≤38℃, the layer thickness is ≤45cm, and the maintenance time is ≥7 days.