Phase change cement composite material and preparation method thereof

By combining the cement connection network with phase change materials, and using heat treatment to form phase change cement composite materials, the problem of insufficient stability of phase change materials in building structure is solved, and high-density and high-strength building materials are achieved, suitable for building construction Energy saving and temperature control applications.

CN118955068AInactive Publication Date: 2024-11-15SHANDONG KONGMING CULTURE MEDIA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411084147.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Phase change materials are insufficiently fixed and stable in building structures, resulting in leakage or dispersion, affecting their performance and service life.

Method used

By combining the cement communication network with the phase change material, a network is formed by using heat treatment to spontaneously fill the phase change material, and a phase change cement composite material with good stability and controllability is prepared. The specific steps include dissolving the acrylic resin and sodium carbonate in a mixed solvent, mixing and stirring with cement, fine river sand, paraffin and quicklime, and then heating in a blower oven to form a phase-change cement composite.

Benefits of technology

This method does not need to consider the wetting and pore connectivity of phase change materials. The preparation process is simple, the material density and strength are high, which avoids leakage of phase change materials and is suitable for building materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955068A_ABST
    Figure CN118955068A_ABST
Patent Text Reader

Abstract

The invention discloses a phase change cement composite material and a preparation method thereof, and relates to the field of cement composite material preparation. The method comprises the following steps: constructing a cement communication network, filling a phase change material, dissolving acrylic resin and sodium carbonate in a mixed solvent of methyl ethyl ketone and acetone according to a mass ratio of 1: (0.05-0.5), sealing, heating and stirring until acrylic acid is completely dissolved; stirring and mixing the obtained gel solution with commercially available cement, fine river sand, paraffin and quick lime in parts by mass, adding water accounting for 10-50% of the total mass, and standing; and finally, heating the material in a blast oven to obtain the phase change cement composite material. When the cement is prepared, the infiltration problem and the hole communication problem of the phase-change material do not need to be considered, the preparation process is simple, only stirring and heat treatment are needed, and industrial preparation is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of cement composite material preparation, and in particular to a phase change cement composite material and a preparation method thereof. Background Art

[0002] With the continuous development of the construction engineering field, the demand for building materials with excellent performance is becoming more and more urgent. Phase change materials, as a new type of material with special properties, can absorb or release a large amount of heat when the temperature changes, so they have broad application prospects in building energy conservation, temperature control and other aspects.

[0003] However, there are some problems in the practical application of phase change materials, such as insufficient fixation and stability in building structures, which can easily cause leakage or dispersion of phase change materials, thus affecting their performance and service life. Therefore, how to combine phase change materials with other building materials to prepare composite materials with good stability and performance has become one of the current research hotspots. Summary of the invention

[0004] In order to solve the above problems, the present invention proposes a method for preparing a phase change cement composite material. The method combines a cement interconnected network with a phase change material, and spontaneously fills the phase change material while forming the network through heat treatment, without considering the uniformity of the filling, and has good stability and controllability. Specifically, the method comprises the following steps:

[0005] Step 1: dissolve acrylic resin and sodium carbonate in a mixed solvent of methyl ethyl ketone and acetone in a mass ratio of 1:0.05-0.5, seal, heat and stir until the acrylic acid is completely dissolved;

[0006] Step 2: The obtained gel solution is mixed with commercially available cement, fine river sand, paraffin and quicklime according to weight proportions, and then 10 to 50% of water is added to the total weight, and then allowed to stand;

[0007] Step 3: heating in a blast oven to obtain a phase change cement composite material.

[0008] In particular, in step one, the ratio of methyl ethyl ketone to acetone is 1:0.5-2, the mass fraction of acrylic resin and sodium carbonate dissolved is 20%-40%, the heating temperature is 40-50 degrees, the stirring rate is 100-500rpm, and the stirring time is 2-3h.

[0009] In particular, in step 2, by mass fraction, the gel solution is 10 to 15 parts, the commercially available cement is 30 to 60 parts, the fine river sand is 15 to 30 parts, the paraffin is 5 to 10 parts, and the quicklime is 10 to 20 parts; the stirring rate is 50 to 300 rpm, the stirring time is 0.5 to 2 hours, and the standing time is 12 to 24 hours.

[0010] Particularly, in step three, the heating temperature of the blast oven is 80 to 120 degrees, and the heating time is 4 to 5 hours.

[0011] The invention further discloses a phase change cement composite material prepared by the preparation method.

[0012] Compared with the prior art, the phase change cement composite material and the preparation method thereof disclosed in the present invention have the following advantages:

[0013] 1. The cement of the present invention does not need to consider the infiltration problem and pore connectivity problem of the phase change material during preparation. The preparation process is simple and only requires stirring and heat treatment, which is conducive to industrial preparation.

[0014] 2. The cement material prepared by the present invention has pores inside, so the phase change material will not leak, has high density and strength, and is very suitable for use as a building material. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions of the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0016] Figure 1 It is a comparison chart of the strength of cement in the embodiment and the comparative example.

[0017] Figure 2 It is a density comparison diagram of cement in the embodiment and the comparative example. DETAILED DESCRIPTION

[0018] The specific implementation of the present invention is briefly described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] Embodiment 1

[0020] The present invention discloses a method for preparing a phase change cement composite material, which comprises the following steps:

[0021] Step 1: Dissolve 20 g of acrylic resin and 4 g of sodium carbonate in a mixed solvent of 100 ml of methyl ethyl ketone and acetone (ratio 1:1.5) at a mass ratio of 1:0.2, seal and heat to 45 degrees, and stir at a stirring rate of 300 rpm for 2.5 hours until the acrylic resin is completely dissolved.

[0022] Step 2: 10 parts of the obtained gel solution, 50 parts of commercially available cement, 20 parts of fine river sand, 8 parts of paraffin and 12 parts of quicklime are mixed according to their weight proportions, and then 30% of water is added to the total weight, stirred at a stirring rate of 200 rpm for 1 hour, and then allowed to stand for 24 hours.

[0023] Step 3: Place the above materials in a forced air oven and heat at 100 degrees for 4.5 hours to obtain a phase change cement composite material.

[0024] Embodiment 2

[0025] The present invention discloses a method for preparing a phase change cement composite material, which comprises the following steps:

[0026] Step 1: Dissolve 30 g of acrylic resin and 15 g of sodium carbonate in a mixed solvent of 150 ml of methyl ethyl ketone and acetone (ratio 1:2) at a mass ratio of 1:0.5, seal and heat to 50 degrees, and stir at a stirring rate of 400 rpm for 3 hours until the acrylic resin is completely dissolved.

[0027] Step 2: Mix 15 parts of the obtained gel solution, 60 parts of commercial cement, 25 parts of fine river sand, 10 parts of paraffin and 15 parts of quicklime according to their weight proportions, then add 40% of water in total weight proportion, stir at a stirring rate of 300 rpm for 1.5 hours, and then let stand for 12 hours.

[0028] Step 3: Place the above materials in a forced air oven and heat at 90 degrees for 4 hours to obtain a phase change cement composite material.

[0029] Embodiment 3

[0030] The present invention discloses a method for preparing a phase change cement composite material, which comprises the following steps:

[0031] Step 1: Dissolve 25 g of acrylic resin and 5 g of sodium carbonate in a mixed solvent of 125 ml of methyl ethyl ketone and acetone (ratio 1:1) in a mass ratio of 1:0.2, seal and heat to 40 degrees, and stir at a stirring rate of 200 rpm for 2 hours until the acrylic resin is completely dissolved.

[0032] Step 2: 12 parts of the obtained gel solution, 40 parts of commercially available cement, 15 parts of fine river sand, 6 parts of paraffin and 10 parts of quicklime are mixed according to their weight proportions, and then 20% of water is added to the total weight, and the mixture is stirred at a stirring rate of 150 rpm for 1 hour, and then allowed to stand for 18 hours.

[0033] Step 3: Place the above materials in a forced air oven and heat at 110 degrees for 5 hours to obtain a phase change cement composite material.

[0034] Comparative Example

[0035] A method for preparing a cement composite material comprises the following steps:

[0036] Step 1: Dissolve 20 g of acrylic resin and 4 g of sodium carbonate in a mixed solvent of 100 ml of methyl ethyl ketone and acetone (ratio 1:1.5) at a mass ratio of 1:0.2, seal and heat to 45 degrees, and stir at a stirring rate of 300 rpm for 2.5 hours until the acrylic resin is completely dissolved.

[0037] Step 2: 10 parts of the obtained gel solution, 50 parts of commercial cement, 20 parts of fine river sand and 12 parts of quicklime were mixed according to the weight ratio, and then 30% of the total weight of water was added, and the mixture was stirred at a stirring rate of 200 rpm for 1 hour, and then allowed to stand for 24 hours. No phase change material paraffin was added.

[0038] Step 3: Place the above materials in a forced air oven and heat at 100 degrees for 4.5 hours to obtain a comparative cement composite material.

[0039] At room temperature of 25 degrees, the strength and density of cement can be significantly improved by adding acrylic resin, sodium carbonate and paraffin, and optimizing the stirring and heating conditions. Figure 1 , 2 As shown, Examples 1, 2, and 3 all exhibit relatively high strength and density, while the comparative example verifies the importance of the phase change material paraffin, whose strength and density are significantly lower, further illustrating the key role of material formulation and processing conditions in cement performance.

[0040] The above description of the disclosed embodiments enables those skilled in the art to implement and use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit and scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest range consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a phase change cement composite material, characterized in that: The method comprises the following steps: constructing a cement interconnected network and then filling the phase change material. Step 1: dissolve acrylic resin and sodium carbonate in a mixed solvent of methyl ethyl ketone and acetone in a mass ratio of 1:0.05-0.5, seal, heat and stir until the acrylic acid is completely dissolved; Step 2: The obtained gel solution is mixed with commercially available cement, fine river sand, paraffin and quicklime according to weight proportions, and then 10 to 50% of water is added to the total weight, and then allowed to stand; Step 3: placing the above materials in a blast oven and heating them to obtain a phase change cement composite material.

2. The method for preparing a phase change cement composite material according to claim 1, characterized in that: In step 1, the ratio of methyl ethyl ketone to acetone is 1:0.5-2, the mass fraction of acrylic resin and sodium carbonate dissolved is 20%-40%, the heating temperature is 40-50 degrees, the stirring rate is 100-500rpm, and the stirring time is 2-3h.

3. The method for preparing a phase change cement composite material according to claim 1, characterized in that: In step 2, by mass fraction, there are 10 to 15 parts of gel solution, 30 to 60 parts of commercial cement, 15 to 30 parts of fine river sand, 5 to 10 parts of paraffin, and 10 to 20 parts of quicklime; the stirring rate is 50 to 300 rpm, the stirring time is 0.5 to 2 h, and the standing time is 12 to 24 h.

4. The method for preparing a phase change cement composite material according to claim 1, characterized in that: In step three, the heating temperature of the blast oven is 80 to 120 degrees, and the heating time is 4 to 5 hours.

5. A phase change cement composite material prepared by the preparation method according to any one of claims 1 to 4.