Preparation method of high-performance conductive aluminum oxide precision ceramic
By optimizing the raw material ratio and sintering process of alumina ceramics, high-performance conductive alumina ceramics are prepared, which solves the problems of high resistivity of the ceramics and coating wear, and realizes the stability of the electrical conductivity and mechanical properties of the ceramics themselves, satisfying high performance, and satisfying high resistance to the ceramics. Accuracy chip process requirements.
Patent Information
- Application Number
- CN202411061436.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
In semiconductor equipment, existing alumina ceramics cannot effectively prevent static electricity due to high resistivity, and coating wear leads to dust pollution, affecting the electrostatic removal effect, and cannot meet the conductivity requirements of high-precision chip processes.
The raw materials with a weight ratio of 80-92.5:5-10:2.5-10 of zinc oxide powder: magnesium oxide: zinc oxide, and sintered by ball milling, single-piece initial pressure, multi-stage heating and pressurization, bidirectional pressurization and vacuum hot pressing In other processes, high-performance conductive alumina precision ceramics are prepared to ensure that the ceramics themselves have electrical conductivity and good mechanical properties.
The prepared high-performance conductive alumina ceramics have uniform and stable resistance, directly have conductive properties, and do not require coating, ensuring stability during the static removal process, maintaining good mechanical properties, and meeting the needs of high-precision chip processes.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and more specifically to a method for preparing high-performance conductive aluminum oxide precision ceramics. Background Art
[0002] In the manufacturing of semiconductor equipment, advanced ceramics play an important role as key component materials. Ceramic robotic arms play a role in handling in semiconductor equipment. They are equivalent to the arms of semiconductor equipment robots and are responsible for transporting wafers or chips to designated locations.
[0003] Alumina ceramics have the physical properties of high density, high hardness, high wear resistance, good heat resistance, excellent mechanical strength, and good corrosion resistance in high temperature environments. They are widely used in semiconductor equipment and are an excellent material for making semiconductor ceramic arms.
[0004] As the manufacturing process precision of 7nm and 5nm chips becomes higher and higher, the demand for conductive precision ceramics is increasing. The main function of conductive precision ceramics is to eliminate static electricity generated during the chip production process and prevent static electricity from affecting chip quality during the manufacturing process. The process currently used abroad is atmospheric pressure sintering of alumina ceramics. Because it is not conductive, it is necessary to apply a conductive coating on its surface. The biggest problem is that the wear and fall of the coating during use will cause dust pollution and affect its anti-static effect, bringing instability to the anti-static production process. The resistivity of most domestically produced alumina is 10 5 Ω -1 ·m -1 The resistivity is high and only meets some anti-static requirements. With the development of technology, the requirements for resistors are becoming more and more diverse.
[0005] Therefore, there is an urgent need for a method for preparing high-performance conductive alumina precision ceramics. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a method for preparing high-performance conductive aluminum oxide precision ceramics to solve the problems in the background technology.
[0007] In order to solve the above technical problems, the technical solutions adopted by the present invention are as follows.
[0008] A method for preparing high-performance conductive aluminum oxide precision ceramics specifically comprises the following steps:
[0009] S1. Take out the raw materials, stabilizer and conductive agent according to the weight ratio and mix them evenly. Then add ethanol as a mixing agent at a volume ratio of 1:1 and ball mill for 14 hours. Pour out, dry and crush through a 300-mesh sieve to obtain a prefabricated powder. Then put the prefabricated powder into a mold and press it into a single piece to obtain a density of 2.4-2.5g / cm 3 of rough stock;
[0010] S2, heating the rough blank obtained in step S1 to 1150-1200°C and keeping it warm for 2 hours, then pressurizing to 20-25 MPa, keeping it under pressure for 2-4 hours, heating it to 1550°C at 1-2°C / min, keeping it under pressure for 3 hours, and increasing the density of the rough blank to 2.9-3.1 g / cm 3 , using a bidirectional pressurization method to pressurize twice to 40-45MPa and maintain the pressure for 5 hours; and performing vacuum hot pressing sintering for 6-8 hours, and then slowly cooling to 1200-1250°C at 0.5-1.1°C / min, releasing the pressure, cooling naturally, and taking out of the furnace after cooling to room temperature, so as to obtain the high-performance conductive alumina precision ceramic blank;
[0011] S3, cutting and grinding the high-performance conductive alumina precision ceramic blank prepared in step S2 to obtain conductive alumina ceramics.
[0012] Further optimize the technical scheme, in step S1, the raw material is alumina powder, the stabilizer is magnesium oxide, the conductive agent is zinc oxide, and the weight ratio is alumina powder: magnesium oxide: zinc oxide = 80-92.5: 5-10: 2.5-10; the purity of the alumina powder is greater than 99.8%, the particle size is less than 1 μm, and the bulk density is 1.0-1.2 g / cm 3 , the shape is spherical.
[0013] To further optimize the technical solution, the ball milling in step S1 uses alumina balls and nylon ball mill jars, and the volume ratio of the mixed solution to the volume of the ball mill jar is 0.8.
[0014] To further optimize the technical solution, the initial pressing pressure of the single piece in step S1 is 60-75 MPa.
[0015] To further optimize the technical solution, the method of heating and pressurizing in step S2 is: heating to 1150-1200°C at 1-2°C / min; pressurizing to 8-12MPa at 0.2-0.4MPa / min, maintaining the pressure at 8-12MPa for 1-2h, and then pressurizing to 20-25MPa at 0.4-0.6MPa / min, maintaining the pressure at 20-25MPa for 2-4h; when pressurizing to 40-45MPa, pressurize at 0.8-1.2MPa / min.
[0016] The technical solution is further optimized, and the sintering rate in step S2 is 1-2°C / min.
[0017] Due to the adoption of the above technical scheme, the technical progress achieved by the present invention is as follows.
[0018] The present invention provides a method for preparing a high-performance conductive alumina precision ceramic, which controls the ratio of alumina powder, stabilizer and conductive agent, adopts ball milling to mix materials, controls the initial pressure, adopts multi-stage temperature rise control, two-way pressurization, controls vacuum hot pressing sintering parameters, cooling rate and pressure relief temperature, etc., to prepare a high-performance conductive alumina precision ceramic with a resistance of 1 to 10 7 Ω, and the resistance is uniform, stable and long-lasting. The ceramic itself is directly conductive and is formed in one piece without any coating. It not only meets the requirements of stable and uniform resistance, but also maintains good mechanical properties, is not afraid of wear, and ensures stability during the static electricity removal process. The present invention effectively ensures the compactness of the high-performance conductive alumina precision ceramics, the uniformity of the conductive properties, and the uniformity of the single-furnace ceramics. The operation of the entire preparation process is safe and controllable, and the uniformity of quality and stability between product batches can be guaranteed in the actual industrial production process, thereby meeting the static electricity removal and stable mechanical property requirements of conductive ceramics, and can realize industrial production. DETAILED DESCRIPTION
[0019] A method for preparing high-performance conductive aluminum oxide precision ceramics specifically comprises the following steps:
[0020] S1. Take out the raw materials, stabilizer and conductive agent according to the weight ratio and mix them evenly.
[0021] The raw material is alumina powder, the purity of which is greater than 99.8%, the particle size is less than 1 μm, and the apparent density is 1.0 to 1.2 g / cm 3 The shape is spherical. The stabilizer is magnesium oxide, the conductive agent is zinc oxide, and the weight ratio of the three is aluminum oxide powder: magnesium oxide: zinc oxide = 90-92.5: 5-6: 2.5-4.
[0022] Ethanol was used as a mixing agent for the powder mixture and added in a volume ratio of 1:1 for 14 hours of ball milling to ensure the uniformity of the conductive precision alumina ceramic resistor. The ball milling used alumina balls and nylon ball milling jars, and the volume ratio of the mixed solution to the volume of the ball milling jar was 0.8.
[0023] After ball milling, pour out, dry, and crush through a 300-mesh sieve to obtain a prefabricated powder.
[0024] The obtained prefabricated powder is loaded into a mold and subjected to a single-piece initial compression at 60-75 MPa to obtain a density of 2.4-2.5 g / cm 3 Rough blank.
[0025] S2, heating the rough blank obtained in step S1 to 1150-1200°C at 1-2°C / min and keeping it warm for 2h, then pressurizing to 8-12MPa at 0.2-0.4MPa / min, keeping it warm for 1-2h, then pressurizing to 20-25MPa at 0.4-0.6MPa / min, keeping it warm for 2-4h; heating to 1550°C at 1-2°C / min, keeping it warm for 3h, and increasing the density of the rough blank to 2.9-3.1g / cm 3 , and then use the bidirectional pressurization method to pressurize the steel sheet to 40-45 MPa at 0.8-1.2 MPa / min for the second time and maintain the pressure for 5 hours; and then perform vacuum hot pressing sintering for 6-8 hours at a sintering rate of 1-2°C / min. The sintering process achieves high-density conductive alumina precision ceramics and ensures its stable mechanical properties.
[0026] The obtained rough blank is sintered and pressurized by multi-stage temperature rise and pressure control and bidirectional pressurization, which ensures that the rough blank is subjected to uniform force and has high density, so that the densification process of the ceramic from top to bottom during vacuum hot pressing sintering is uniform and stable.
[0027] Then slowly cool down to 1200-1250°C at 0.5-1.1°C / min, release the pressure, cool naturally, and take out of the furnace after cooling to room temperature, which can further improve the density and uniformity of the alumina; thus, the high-performance conductive alumina precision ceramic blank is obtained.
[0028] S3, cutting and grinding the high-performance conductive alumina precision ceramic blank prepared in step S2 to obtain conductive alumina ceramics.
[0029] The present invention will be further described in detail below with reference to specific embodiments.
[0030] Embodiment 1:
[0031] A method for preparing high-performance conductive aluminum oxide precision ceramics specifically comprises the following steps:
[0032] S1, purity> 99.8%, particle size < 1μm, bulk density 1.0~1.2g / cm 3 , 1935g of spherical alumina powder. Take 129g of magnesium oxide as stabilizer and 86g of zinc oxide as conductive agent, add 2100mL of ethanol as a mixture, and ball mill for 14h. Pour out after ball milling, dry, crush and pass through a 300-mesh sieve to obtain prefabricated powder.
[0033] The obtained prefabricated powder was loaded into the mold and subjected to 75MPa single-piece initial pressing to obtain a rough blank with a thickness of 86mm, a mold size of 100mm (length)*100mm (width)*300 (height)mm, and a density of 2.5g / cm 3 Rough blank.
[0034] S2, put the rough blank obtained in step S1 into a vacuum hot pressing sintering furnace, heat it to 1150℃ at 2℃ / min and keep it warm for 2h, then pressurize it to 8MPa at 0.2MPa / min, keep it warm for 1h, then pressurize it to 25MPa at 0.6MPa / min, keep it warm for 2h; heat it to 1550℃ at 1℃ / min, keep it warm for 3h, at this time, the rough blank stroke drops by 12.2mm, and the rough blank density is calculated to be 2.95g / cm 3 .
[0035] Then, the double-direction pressurization method is adopted to pressurize the steel sheet to 40MPa at 1.2MPa / min for a second time and maintain the pressure for 5h; and vacuum hot pressing sintering is performed for 8h, and the sintering rate is 1℃ / min. Then, the steel sheet is slowly cooled to 1200℃ at 1.1℃ / min, the pressure is released, the temperature is naturally cooled, and the steel sheet is taken out of the furnace after cooling to room temperature, thereby obtaining the high-performance conductive alumina precision ceramic blank.
[0036] S3, cutting and grinding the high-performance conductive alumina precision ceramic blank prepared in step S2 to obtain conductive alumina ceramic. The density of conductive alumina ceramic is 3.98 g / cm 3 , surface resistance 10 6-7 Ω, flexural strength 520MPa, elastic modulus 372GPa. After 30 days, the surface resistance is still 10 6-7 Ω, no attenuation occurs.
[0037] Embodiment 2:
[0038] A method for preparing high-performance conductive aluminum oxide precision ceramics specifically comprises the following steps:
[0039] S1, purity> 99.8%, particle size < 1μm, bulk density 1.0~1.2g / cm 3 , 1999g of spherical alumina powder. Take 112g of magnesium oxide as stabilizer and 89g of zinc oxide as conductive agent, add 2200mL of ethanol as a mixture, and ball mill for 14h. Pour out after ball milling, dry, crush through a 300-mesh sieve, and obtain prefabricated powder.
[0040] The obtained prefabricated powder was loaded into the mold and subjected to 60MPa single-piece initial pressing to obtain a rough blank with a thickness of 94mm, a mold size of 100mm (length)*100mm (width)*300 (height)mm, and a density of 2.5g / cm 3 Rough blank.
[0041] S2, the rough blank obtained in step S1 is loaded into a vacuum hot pressing sintering furnace, and the temperature is raised to 1180°C at 1.5°C / min and kept at this temperature for 2h, and then pressurized to 10MPa at 0.4MPa / min, kept at this temperature for 1h, and then pressurized to 25MPa at 0.5MPa / min, kept at this temperature for 2h; the temperature is raised to 1550°C at 1.5°C / min, kept at this temperature for 3h, at which time the rough blank travel drops by 12mm, and the rough blank density is calculated to be 2.90g / cm 3 .
[0042] Then, the pressure was increased to 42MPa at 0.8MPa / min by bidirectional pressure and maintained for 5h; vacuum hot pressing sintering was performed for 6h, and the sintering rate was 1℃ / min. Then, the temperature was slowly reduced to 1180℃ at 1.1℃ / min, the pressure was released, the temperature was naturally reduced, and the temperature was removed from the furnace after being reduced to room temperature, thus obtaining the high-performance conductive alumina precision ceramic blank.
[0043] S3, cutting and grinding the high-performance conductive alumina precision ceramic blank prepared in step S2 to obtain conductive alumina ceramic. The density of conductive alumina ceramic is 3.95 g / cm 3 , surface resistance 10 5-6 Ω, flexural strength 552MPa, elastic modulus 370GPa. After 45 days, the surface resistance was 10 5-6 Ω, no attenuation occurs.
[0044] Embodiment 3:
[0045] A method for preparing high-performance conductive aluminum oxide precision ceramics specifically comprises the following steps:
[0046] S1, purity> 99.8%, particle size < 1μm, bulk density 1.0~1.2g / cm 3 , 4000g of spherical alumina powder. Take 500g of magnesium oxide as stabilizer and 500g of zinc oxide as conductive agent, and use 5200mL of ethanol as a mixture, and ball mill for 14h. Pour out after ball milling, dry, crush and pass through a 300-mesh sieve to obtain prefabricated powder.
[0047] The obtained prefabricated powder was loaded into the mold and subjected to 70MPa single-piece initial pressing to obtain a rough blank with a thickness of 204mm, a mold size of 100mm (length)*100mm (width)*300 (height)mm, and a density of 2.45g / cm 3 Rough blank.
[0048] S2, the rough blank obtained in step S1 is loaded into a vacuum hot pressing sintering furnace, and the temperature is raised to 1200°C at 1°C / min and kept at this temperature for 2 hours, and then pressurized to 12MPa at 0.3MPa / min, kept at this temperature for 1 hour, and then pressurized to 23MPa at 0.4MPa / min, kept at this temperature for 3 hours; the temperature is raised to 1550°C at 2°C / min, kept at this temperature for 3 hours, at which time the rough blank travel drops by 11.2mm, and the rough blank density is calculated to be 2.93g / cm 3 .
[0049] Then, the double-direction pressurization method is adopted to pressurize the steel sheet to 45MPa at 1.1MPa / min for a second time and maintain the pressure for 5h; and vacuum hot pressing sintering is performed for 7h, and the sintering rate is 1.5℃ / min. Then, the temperature is slowly reduced to 1250℃ at 0.8℃ / min, the pressure is released, the temperature is naturally reduced, and the steel sheet is taken out of the furnace after being cooled to room temperature, thereby obtaining the high-performance conductive alumina precision ceramic blank.
[0050] S3, cutting and grinding the high-performance conductive alumina precision ceramic blank prepared in step S2 to obtain conductive alumina ceramic. The density of conductive alumina ceramic is 3.96 g / cm 3 , surface resistance 1~5Ω, flexural strength 498MPa, elastic modulus 372GPa. After 80 days, the surface resistance was 1~5Ω, and no attenuation occurred.
[0051] Embodiment 4:
[0052] A method for preparing high-performance conductive alumina precision ceramics, when mass-producing large-size high-performance conductive alumina precision ceramics, specifically comprises the following steps:
[0053] S1, purity> 99.8%, particle size < 1μm, bulk density 1.0~1.2g / cm 3 , 15015g of spherical alumina powder. Take 825g of magnesium oxide as stabilizer and 660g of zinc oxide as conductive agent, mix them with 16500mL of ethanol as a mixing agent for 5 times, and ball mill for 14 hours. Pour out after ball milling, dry, crush and pass through a 300-mesh sieve to obtain prefabricated powder.
[0054] The obtained prefabricated powder was loaded into the mold and subjected to 70MPa single-piece initial pressing to obtain a rough blank with a thickness of 74.5mm, a mold size of 300mm (length)*300mm (width)*0.9 (height)mm*5 pieces, and a density of 2.46g / cm 3 Rough blank.
[0055] S2, the rough blank obtained in step S1 is loaded into a vacuum hot pressing sintering furnace, and the temperature is raised to 1200°C at 1°C / min and kept at this temperature for 2 hours, and then pressurized to 12MPa at 0.3MPa / min, and kept at this temperature for 1 hour, and then pressurized to 23MPa at 0.4MPa / min, and kept at this temperature for 1.5 hours; the temperature is raised to 1550°C at 2°C / min, and kept at this temperature for 3 hours. At this time, the rough blank travel drops by 11.2mm. After calculation, the rough blank density is 2.93g / cm 3 .
[0056] Then, the double-direction pressurization method is adopted to pressurize the steel sheet to 45MPa at 1.1MPa / min for a second time and maintain the pressure for 5h; and vacuum hot pressing sintering is performed for 7h, and the sintering rate is 1.5℃ / min. Then, the temperature is slowly reduced to 1250℃ at 0.8℃ / min, the pressure is released, the temperature is naturally reduced, and the steel sheet is taken out of the furnace after being cooled to room temperature, thereby obtaining the high-performance conductive alumina precision ceramic blank.
[0057] S3, cutting and grinding the high-performance conductive alumina precision ceramic blank prepared in step S2 to obtain conductive alumina ceramic. The density of conductive alumina ceramic is 3.98 g / cm 3 , surface resistance 10 5-6 Ω, flexural strength 588MPa, elastic modulus 372GPa; and the large ceramic resistance is uniform and the appearance is consistent; and the SEM magnification 5000 times detection shows that the resistance structure is compact, without pores, and has good density. After 100 days, the surface resistance is 105-6Ω, and there is no attenuation.
[0058] In summary, it can be seen that the resistance of the high-performance conductive alumina precision ceramics prepared under the process conditions of the present invention can reach 1 to 10 7 Ω, and the resistance is uniform and stable. Ceramic density ≥3.95g / cm 3 , high density, flexural strength ≥480MPa, elastic modulus ≥360GPa, excellent mechanical properties, and the conductive alumina precision ceramics have no pores, no defects, and consistent appearance; moreover, the quality of the product can be guaranteed during mass production.
Claims
1. A method for preparing high-performance conductive alumina precision ceramics, characterized in that: The specific steps include: S1. Take out the raw materials, stabilizer and conductive agent according to the weight ratio and mix them evenly. Then add ethanol as a mixing agent at a volume ratio of 1:1 and ball mill for 14 hours. Pour out, dry and crush through a 300-mesh sieve to obtain a prefabricated powder. Then put the prefabricated powder into a mold and press it into a single piece to obtain a density of 2.4-2.5g / cm 3 of rough stock; S2, heating the rough blank obtained in step S1 to 1150-1200°C and keeping it warm for 2 hours, then pressurizing to 20-25 MPa, keeping it under pressure for 2-4 hours, heating it to 1550°C at 1-2°C / min, keeping it under pressure for 3 hours, and increasing the density of the rough blank to 2.9-3.1 g / cm 3 , using a bidirectional pressurization method to pressurize twice to 40-45MPa and maintain the pressure for 5 hours; and performing vacuum hot pressing sintering for 6-8 hours, and then slowly cooling to 1200-1250°C at 0.5-1.1°C / min, releasing the pressure, cooling naturally, and taking out of the furnace after cooling to room temperature, so as to obtain the high-performance conductive alumina precision ceramic blank; S3, cutting and grinding the high-performance conductive alumina precision ceramic blank prepared in step S2 to obtain conductive alumina ceramics.
2. The method for preparing a high-performance conductive alumina precision ceramic according to claim 1, characterized in that: In step S1, the raw material is alumina powder, the stabilizer is magnesium oxide, the conductive agent is zinc oxide, and the weight ratio is alumina powder: magnesium oxide: zinc oxide = 80-92.5: 5-10: 2.5-10; the purity of the alumina powder is greater than 99.8%, the particle size is less than 1 μm, and the bulk density is 1.0-1.2 g / cm 3 , the shape is spherical.
3. The method for preparing a high-performance conductive alumina precision ceramic according to claim 1, characterized in that: The ball milling in step S1 uses alumina balls and a nylon ball mill jar, and the volume ratio of the mixed solution to the volume of the ball mill jar is 0.
8.
4. The method for preparing a high-performance conductive alumina precision ceramic according to claim 1, characterized in that: The initial pressing pressure of the single sheet in step S1 is 60-75 MPa.
5. The method for preparing a high-performance conductive alumina precision ceramic according to claim 4, characterized in that: The method of heating and pressurizing in step S2 is: heating to 1150-1200° C. at 1-2° C. / min; pressurizing to 8-12 MPa at 0.2-0.4 MPa / min, maintaining the pressure at 8-12 MPa for 1-2 hours, and then pressurizing to 20-25 MPa at 0.4-0.6 MPa / min, maintaining the pressure at 20-25 MPa for 2-4 hours; when pressurizing to 40-45 MPa, pressurizing at 0.8-1.2 MPa / min.
6. The method for preparing a high-performance conductive alumina precision ceramic according to claim 1, characterized in that: The sintering rate in step S2 is 1-2°C / min.
Citation Information
Patent Citations
Nanostructure composite LED (Light Emitting Diode) ceramic substrate and manufacturing method thereof
CN102821550A
Porous alumina ceramics, as well as preparation method and application thereof
CN107200599A
Preparation method of tungsten sulfide target material
CN108585868A
Method for producing aluminium oxide base nano complex phase ceramics
CN1099016A
Multiphase ceramic material and preparation method thereof