Epoxy vegetable oil glass polymer material and preparation method thereof

Through solvent-free one-pot melt polymerization technology, epoxy vegetable oil, aldehyde compounds and diamines react under a catalyst, the problem of resource dependence and environmental pollution of traditional epoxy resins is solved, and the epoxy vegetable oil glass polymers is realized. Efficient, environmentally friendly, low-cost preparation, suitable for a variety of application needs.

CN118955834AActive Publication Date: 2024-11-15SOUTHWEST UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411027379.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The raw materials of traditional epoxy resins are derived from fossil resources, resulting in resource depletion and environmental pollution. There are many reaction steps for preparing epoxy vegetable oil glass polymers and use solvents, which increases costs and pollution risks.

Method used

The solvent-free one-pot melt polymerization is used to react epoxy vegetable oil, aldehyde compounds containing phenolic hydroxyl or carboxyl groups and diamines in the presence of a catalyst. Through the activity differences between functional groups, the preparation of epoxy vegetable oil glass polymers is achieved. , simplify process flow and reduce costs.

Benefits of technology

It has achieved efficient preparation of epoxy vegetable oil glass polymers, which has the characteristics of green and environmental protection, low cost and flexible structural control, avoids solvent treatment and pollution, and is suitable for different application fields.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an epoxy vegetable oil glass high polymer material and a preparation method thereof, the epoxy vegetable oil glass high polymer material is obtained by taking epoxy vegetable oil, aldehyde compounds containing phenolic hydroxyl groups or / and carboxyl groups and diamine as raw materials, and reacting in the presence of a catalyst at 130-200 DEG C in a nitrogen atmosphere. The novel solvent-free one-pot method for preparing the epoxy vegetable oil glass polymer material is designed by utilizing the reaction activity difference between functional groups, no solvent is needed in the preparation process, tedious steps such as product purification and solvent treatment are omitted, and the method has the characteristics of high efficiency, low cost, no pollution and the like. The preparation method has universality, and the structure and performance of the epoxy vegetable oil glass polymer material can be regulated and controlled in a relatively large range by selecting aldehyde group-containing compounds and diamine with different structures, so that the requirements of different application fields are met. In addition, the preparation method provided by the invention is simple and convenient to operate, does not need to use special instruments and equipment, and is high in operability and economical.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to an epoxy vegetable oil glass polymer material and a preparation method thereof. Background Art

[0002] Epoxy resin is a type of thermosetting plastic with excellent dimensional stability, mechanical strength, heat resistance and chemical corrosion resistance. It has been widely used in adhesives, insulating materials, electronic packaging and composite materials. However, the raw materials of traditional epoxy resins are derived from fossil resources, and the permanent cross-linked network structure makes it difficult to recycle after use. The development of epoxy resins faces the problems of resource depletion and environmental pollution. Therefore, the development of sustainable epoxy resins has become an urgent need. On the one hand, using renewable biomass as raw materials to prepare bio-based epoxy resins can solve the problem of epoxy resin's dependence on fossil resources. On the other hand, dynamic covalent bonds are introduced into thermosetting epoxy resins to prepare epoxy glass polymers. The exchange reaction of dynamic covalent bonds can give thermosetting epoxy resins thermoplasticity and recyclability. Therefore, the development of bio-based epoxy glass polymer materials provides a way to simultaneously solve the resource crisis and environmental pollution problems faced by epoxy resins.

[0003] Epoxy vegetable oil is a type of bio-based epoxy monomer prepared by epoxidation of vegetable oil containing double bonds. It can undergo curing reactions with carboxylic acids, anhydrides, amines and phenolic compounds to prepare bio-based epoxy resins. By introducing dynamic covalent bonds such as imine bonds, disulfide bonds or borate bonds into epoxy vegetable oil resins, bio-based epoxy glass polymers that can be thermoplastically processed and easily recycled can be obtained. Imine bonds have been widely used in epoxy glass polymers due to their advantages such as easy preparation, exchange without catalysts and controllable structure. At present, there are two main methods for introducing imine bonds into epoxy vegetable oil resins to prepare epoxy vegetable oil glass polymers. One is to first synthesize a dynamic curing agent containing imine bonds and cure it with epoxy vegetable oil to obtain epoxy vegetable oil glass polymers; the other is to use aldehyde-containing compounds to react with epoxy vegetable oil to prepare epoxy vegetable oil polyaldehydes, and then undergo aldehyde-amine condensation reaction with diamines to obtain epoxy vegetable oil glass polymers. However, these two methods have many reaction steps and usually use solvents. The removal and residue of solvents will lead to problems such as increased costs and environmental pollution. Summary of the invention

[0004] In order to solve the above technical problems, the first purpose of the present invention is to provide a method for preparing an epoxy vegetable oil glass polymer material, and the second purpose is to provide an epoxy vegetable oil glass polymer material prepared by the method. The present invention adopts a solvent-free one-pot melt polymerization, which is simple in process, green and environmentally friendly, and economical, and can easily regulate the structure and performance of the vegetable oil epoxy glass polymer.

[0005] To achieve the above first purpose, the present invention is implemented by the following technical scheme: a method for preparing an epoxy vegetable oil-based glass polymer material, characterized in that: epoxy vegetable oil, aldehyde compounds containing phenolic hydroxyl groups and / or carboxyl groups, and diamine are used as raw materials, and reacted at 130-200°C in a nitrogen atmosphere in the presence of a catalyst to obtain the glass polymer material.

[0006] Since the activity of the epoxy bond of epoxidized vegetable oil in reacting with amino group is low, while the activity of the reaction of amino group with aldehyde group and the reaction of another functional group (carboxyl group or phenolic hydroxyl group) of aldehyde compounds containing hydroxyl group or / and carboxyl group with epoxy bond are both high, when the three substances are reacted in one pot, the main reactions occur between amino group and aldehyde group (forming imine bond) and the reaction between another functional group (carboxyl group or phenolic hydroxyl group) and epoxy. Due to the strict control of the raw material ratio, the side reaction of the low-activity amino-epoxy reaction to form a permanent cross-linked structure can be basically ignored. Therefore, the successful preparation of epoxy vegetable oil glass polymer can be achieved by the solvent-free one-pot method. This preparation method does not require solvent and has the characteristics of being green, environmentally friendly and low-cost.

[0007] In the above scheme: the epoxidized vegetable oil is any one or more of epoxidized soybean oil, epoxidized tung oil and epoxidized linseed oil.

[0008] In the above scheme: the aldehyde compound containing phenolic hydroxyl group and / or carboxyl group is any one of vanillin, 4-hydroxybenzaldehyde, 3-hydroxybenzaldehyde, 2-carboxybenzaldehyde and 3-carboxybenzaldehyde.

[0009] In the above scheme: the aldehyde compound containing phenolic hydroxyl group and / or carboxyl group and the epoxy vegetable oil are added according to the molar ratio of phenolic hydroxyl group and / or carboxyl group to epoxy group of 0.5:1.0-1.0:1.0.

[0010] In the above scheme: the diamine is any one of decanediamine, dimeramine, p-phenylenediamine, diphenylmethanediamine, isophoronediamine, and dicyclohexylmethanediamine.

[0011] In the above scheme: the aldehyde compound containing phenolic hydroxyl group and / or carboxyl group and the diamine are added according to the aldehyde group / amino group molar ratio of 1:1.

[0012] In the above scheme: the catalyst is any one of 1-methylimidazole, 2-methylimidazole, 1,2-dimethylimidazole and 4-dimethylaminopyridine.

[0013] In the above scheme: the amount of the catalyst used is 0.01-1% of the total mass of the epoxy vegetable oil, the aldehyde compound containing phenolic hydroxyl and / or carboxyl groups and the diamine.

[0014] In the above scheme: reaction time is 1-12h.

[0015] An epoxidized vegetable oil glass polymer material prepared by the preparation method of the epoxidized vegetable oil glass polymer material.

[0016] Beneficial effects: The present invention utilizes the difference in reaction activity between functional groups to design a new method for preparing epoxy vegetable oil glass polymer materials in a one-pot solvent-free method. The preparation process does not require a solvent, and cumbersome steps such as product purification and solvent treatment are omitted. It has the characteristics of high efficiency, low cost, and no pollution. The preparation method has universal applicability. By selecting aldehyde-containing compounds and diamines of different structures, the structure and performance of epoxy vegetable oil glass polymer materials can be regulated in a large range to meet the needs of different application fields. In addition, the preparation method provided by the present invention is simple to operate, does not require the use of special instruments and equipment, has strong operability, and is economical. DETAILED DESCRIPTION

[0017] The present invention will be further described below in conjunction with the embodiments.

[0018] Example 1

[0019] Epoxidized soybean oil, vanillin and decanediamine are added into a reaction bottle at a phenolic hydroxyl group / epoxy group molar ratio of 0.7:1 and an aldehyde group / amino group molar ratio of 1:1. Epoxidized vegetable oil, aldehyde compounds containing phenolic hydroxyl groups and / or carboxyl groups, and 0.1% of the total mass of the diamine catalyst 1-methylimidazole are added, and the mixture is reacted at 130° C. under a nitrogen atmosphere for 12 hours to obtain an epoxidized vegetable oil glass polymer material.

[0020] Performance Testing

[0021] The obtained epoxidized vegetable oil glass polymer was hot-pressed at 160°C and 10 MPa for 10 minutes by a molding method to obtain an epoxidized vegetable oil glass polymer sheet. The tensile strength of the epoxidized vegetable oil glass polymer was measured according to GB1040-92 standard to be 4.7±0.6MPa, and the elongation at break was 117±7%. The gel fraction was measured using N,N-dimethylformamide to be 90.5%.

[0022] Example 2

[0023] Epoxidized linseed oil, 4-hydroxybenzaldehyde and p-phenylenediamine were added into a reaction bottle at a phenolic hydroxyl group / epoxy group molar ratio of 0.5:1 and an aldehyde group / amino group molar ratio of 1:1, and 0.01% of the total mass of epoxy vegetable oil, aldehyde compounds containing phenolic hydroxyl groups and / or carboxyl groups and diamine as a catalyst 1,2-dimethylimidazole were added, and the mixture was reacted at 150° C. under a nitrogen atmosphere for 10 hours to obtain an epoxy vegetable oil-based glass polymer material.

[0024] Performance Testing

[0025] The obtained epoxidized vegetable oil glass polymer was hot-pressed at 160°C and 10 MPa for 10 minutes by a molding method to obtain an epoxidized vegetable oil glass polymer sheet. The tensile strength of the epoxidized vegetable oil glass polymer was measured according to GB1040-92 standard to be 25.3±0.2MPa, and the elongation at break was 12±3%; the gel fraction was measured using N,N-dimethylformamide to be 93.4%.

[0026] Example 3

[0027] Epoxy tung oil, 3-carboxybenzaldehyde and diphenylmethanediamine were added into a reaction bottle at a carboxyl / epoxy molar ratio of 1:1 and an aldehyde / amino molar ratio of 1:1, and epoxy vegetable oil, aldehyde compounds containing phenolic hydroxyl groups and / or carboxyl groups and 1% of the total mass of diamine catalyst 4-dimethylaminopyridine were added, and the mixture was reacted at 200° C. in a nitrogen atmosphere for 1 hour to obtain an epoxy vegetable oil glass polymer material.

[0028] Performance Testing

[0029] The obtained epoxidized vegetable oil glass polymer was hot-pressed at 160°C and 10 MPa for 10 minutes by a molding method to obtain an epoxidized vegetable oil glass polymer sheet. The tensile strength of the epoxidized vegetable oil glass polymer was measured according to GB1040-92 standard to be 38.7±0.5 MPa, and the elongation at break was 8±2%. The gel fraction was measured using N,N-dimethylformamide to be 95.4%.

[0030] Example 4

[0031] Epoxidized soybean oil, 2-carboxybenzaldehyde and dimeramine are added into a reaction bottle at a carboxyl / epoxy molar ratio of 0.8:1 and an aldehyde / amino molar ratio of 1:1, and epoxy vegetable oil, aldehyde compounds containing phenolic hydroxyl groups and / or carboxyl groups and 0.5% of the total mass of the diamine as a catalyst 2-methylimidazole are added, and the mixture is reacted at 170° C. under a nitrogen atmosphere for 5 hours to obtain an epoxy vegetable oil-based glass polymer material.

[0032] Performance Testing

[0033] The epoxy vegetable oil glass polymer obtained was hot-pressed at 160°C and 10 MPa for 10 minutes by a molding method to obtain an epoxy vegetable oil glass polymer sheet. The tensile strength of the epoxy vegetable oil glass polymer was measured according to GB1040-92 standard to be 15.5±2.3MPa, and the elongation at break was 185±12%; the gel fraction was measured using N,N-dimethylformamide to be 93.8%.

[0034] Example 5

[0035] Epoxy tung oil, 4-hydroxybenzaldehyde and dicyclohexylmethanediamine were added into a reaction bottle at a phenolic hydroxyl group / epoxy group molar ratio of 0.6:1 and an aldehyde group / amino group molar ratio of 1:1, and epoxy vegetable oil, aldehyde compounds containing phenolic hydroxyl groups and / or carboxyl groups and 0.3% of the total mass of the diamine catalyst 1,2-dimethylimidazole were added, and the mixture was reacted at 180° C. in a nitrogen atmosphere for 3 hours to obtain an epoxy vegetable oil-based glass polymer material.

[0036] Performance Testing

[0037] The obtained epoxidized vegetable oil glass polymer was hot-pressed at 160°C and 10 MPa for 10 minutes by a molding method to obtain an epoxidized vegetable oil glass polymer sheet. The tensile strength of the epoxidized vegetable oil glass polymer was measured according to GB1040-92 standard to be 37.6±1.9 MPa, and the elongation at break was 9±3%; the gel fraction was measured using N,N-dimethylformamide to be 85.7%.

[0038] Example 6

[0039] Epoxidized linseed oil, 3-hydroxybenzaldehyde and isophorone diamine were added into a reaction bottle at a phenolic hydroxyl group / epoxy group molar ratio of 0.8:1 and an aldehyde group / amino group molar ratio of 1:1, and epoxy vegetable oil, aldehyde compounds containing phenolic hydroxyl groups and / or carboxyl groups and 0.05% of the total mass of the diamine catalyst 4-dimethylaminopyridine were added, and the mixture was reacted at 140° C. under a nitrogen atmosphere for 10 hours to obtain an epoxy vegetable oil-based glass polymer material.

[0040] Performance Testing

[0041] The obtained epoxidized vegetable oil glass polymer was hot-pressed at 160°C and 10 MPa for 10 minutes by a molding method to obtain an epoxidized vegetable oil glass polymer sheet. The tensile strength of the epoxidized vegetable oil glass polymer was measured according to GB1040-92 standard to be 25.3±0.2MPa, and the elongation at break was 12±3%; the gel fraction was measured using N,N-dimethylformamide to be 93.4%.

[0042] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing epoxy vegetable oil glass polymer material, Features: The epoxidized vegetable oil, aldehyde compounds containing phenolic hydroxyl groups and / or carboxyl groups, and diamine are used as raw materials, and reacted at 130-200° C. in a nitrogen atmosphere in the presence of a catalyst to obtain the epoxidized vegetable oil.

2. The method for preparing the epoxy vegetable oil glass polymer material according to claim 1, Features: The epoxidized vegetable oil is any one or more of epoxidized soybean oil, epoxidized tung oil and epoxidized linseed oil.

3. The method for preparing the epoxy vegetable oil glass polymer material according to claim 2, Features: The aldehyde compound containing phenolic hydroxyl group and / or carboxyl group is any one of vanillin, 4-hydroxybenzaldehyde, 3-hydroxybenzaldehyde, 2-carboxybenzaldehyde and 3-carboxybenzaldehyde.

4. The method for preparing the epoxy vegetable oil glass polymer material according to claim 3, Features: The aldehyde compound containing phenolic hydroxyl group and / or carboxyl group and the epoxy vegetable oil are added according to the molar ratio of phenolic hydroxyl group and / or carboxyl group to epoxy group of 0.5:1.0-1.0:1.

0.

5. The method for preparing the epoxy vegetable oil glass polymer material according to any one of claims 1 to 4, Features: The diamine is any one of decanediamine, dimeramine, p-phenylenediamine, diphenylmethanediamine, isophoronediamine, and dicyclohexylmethanediamine.

6. The method for preparing the epoxy vegetable oil glass polymer material according to claim 5, Features: The aldehyde compound containing phenolic hydroxyl group and / or carboxyl group and the diamine are added according to the aldehyde group / amino group molar ratio of 1:

1.

7. The method for preparing the epoxy vegetable oil glass polymer material according to claim 5, Features: The catalyst is any one of 1-methylimidazole, 2-methylimidazole, 1,2-dimethylimidazole and 4-dimethylaminopyridine.

8. The method for preparing the epoxy vegetable oil glass polymer material according to claim 7, Features: The amount of the catalyst used is 0.01-1% of the total mass of the epoxy vegetable oil, the aldehyde compound containing phenolic hydroxyl or / and carboxyl and the diamine.

9. The method for preparing the epoxy vegetable oil glass polymer material according to claim 1, Features: Reaction time 1-12h.

10. An epoxy vegetable oil glass polymer material prepared by the method for preparing an epoxy vegetable oil glass polymer material according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Biomass-based recoverable epoxy resin as well as preparation method and application thereof

    CN109777040A

  • Thermostable benzoxazine resin compound and its preparation method and uses

    CN1884376A

  • Epoxy resin composition, its cured product, semiconductor sealing material and semiconductor device

    JP2007269979A

  • Vegetable oil-derived epoxy compositions having improved performance

    US20210371579A1