Preparation method of polyurethane composite material with high heat conductivity coefficient
Through the strong acid modification of carbon nanotubes and the directional arrangement of magnetic field, combined with thermal conductivity monitoring, the problem of lack of monitoring in the preparation of polyurethane composite materials is solved, and the thermal conductivity and preparation efficiency of the material are improved.
Patent Information
- Application Number
- CN202411450078.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-17
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The preparation process of polyurethane composites lacks monitoring, resulting in low preparation efficiency and it is impossible to determine whether the performance of the final material is optimal.
By performing strong acid modification treatment on carbon nanotubes, its hydrophilicity and reactivity are increased, and a magnetic field is applied in the polyurethane dispersion to arrange the carbon nanotubes in a directional manner to form a high thermal conductivity channel, combining thermal conductivity monitoring and magnetic field environment adjustment, Ensure that the preparation process of the material meets the standards.
The thermal conductivity and preparation efficiency of polyurethane composite materials are improved, the monitoring accuracy of the preparation process is enhanced, and the optimization of material performance is ensured.
Smart Images

Figure CN118955839A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of polyurethane composite materials, and in particular to a method for preparing a polyurethane composite material with high thermal conductivity. Background Art
[0002] In the rapidly developing field of science and technology, especially in the electronic packaging, thermal management system and new energy vehicle industries, unprecedented high standards are being set for the thermal conductivity of materials. Traditional polyurethane materials, with their excellent mechanical properties, wear resistance and processability, occupy an important position in many fields, but their relatively low thermal conductivity limits their application in scenarios with high heat dissipation requirements.
[0003] In order to solve this technical bottleneck, the scientific research community and the industrial community have begun to work on the development of polyurethane composite materials with high thermal conductivity. The research and development background of such materials is rooted in the growing market demand for high-efficiency thermal conductive materials, aiming to achieve a significant improvement in thermal management efficiency through innovations in materials science and engineering technology. Researchers introduce high thermal conductivity fillers (such as graphene nanosheets, boron nitride powder, metal oxides, etc.) into the polyurethane matrix, and use the excellent thermal conductivity of these fillers to construct an effective thermal conductive network. At the same time, by optimizing the dispersion technology of the filler, adjusting the interface interaction between the matrix and the filler, and improving the polymerization process, it is ensured that the composite material does not sacrifice other key properties such as mechanical strength, weather resistance and processing performance while improving the thermal conductivity.
[0004] Chinese patent publication number: CN105238034A discloses a carbon nanotube modified polyurethane composite material. The raw materials include: terminal hydroxyl polybutadiene, diphenylmethylene diisocyanate, polyisocyanurate, vinyl triethoxysilane, silane coupling agent KH-560, hydroquinone bishydroxyethyl ether, dimethylthiotoluenediamine, dibutyltin dilaurate, polyvinyl chloride, acrylonitrile-styrene-butadiene copolymer, nano calcium carbonate, carbon nanotubes, organic modified montmorillonite, nano silicon dioxide, nano barium titanate, calcium sulfate whisker, dioctyl phthalate, tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester, polybenzimidazole. The carbon nanotube modified polyurethane composite material proposed by the invention has good water resistance, high strength, excellent heat resistance and aging resistance.
[0005] It can be seen that the carbon nanotube-modified polyurethane composite material has the following problems: the invention lacks monitoring of the preparation process of the polyurethane composite material and cannot determine whether the performance of the final composite material is optimal, resulting in low preparation efficiency of the polyurethane composite material. Summary of the invention
[0006] To this end, the present invention provides a method for preparing a polyurethane composite material with high thermal conductivity, so as to overcome the problem in the prior art that the preparation process of the polyurethane composite material is lack of monitoring, thereby resulting in low preparation efficiency of the polyurethane composite material.
[0007] To achieve the above object, the present invention provides a method for preparing a polyurethane composite material with high thermal conductivity, comprising: Step S1, ultrasonically dispersing the washed carbon nanotubes in a solvent to form a dispersion, adding a strong acid mixture to the dispersion for heating and reflux treatment, filtering after refluxing for a preset time to obtain a filtrate, treating the filtrate and drying it to obtain modified carbon nanotubes; Step S2, respectively adding the dehydrated polyol and isocyanate to a first reaction kettle, adding a first catalyst under nitrogen protection to generate a prepolymer, periodically detecting the NCO value to determine whether to stop generating the prepolymer, and adding a hydrophilic chain extender, a crosslinking agent and a stabilizer under the condition of stopping generating the prepolymer to generate a polyurethane dispersion; Step S3, adding the modified carbon nanotubes and the polyurethane dispersion into a second reactor in a preset ratio, placing the second reactor in a magnetic field environment after ultrasonic dispersion, and adding a second catalyst to generate a polyurethane composite material with a high thermal conductivity; Step S4, obtaining the thermal conductivity of the polyurethane composite material, determining whether the preparation process of the polyurethane composite material meets the standard based on the thermal conductivity, obtaining a microscopic distribution image of the modified carbon nanotubes based on the preparation process of the polyurethane composite material that does not meet the standard, determining whether the arrangement direction of a single modified carbon nanotube meets the standard based on the inclination angle of the single modified carbon nanotube, counting the number ratio of the modified carbon nanotubes whose arrangement direction meets the standard and determining whether the setting of the magnetic field environment meets the standard based on the number ratio, and, under the condition that the magnetic field environment meets the standard, adjusting the aspect ratio of the carbon nanotubes based on the thermal conductivity difference, and under the condition that the magnetic field environment does not meet the standard, adjusting the setting parameters of the magnetic field environment based on the inclination angle difference, wherein the setting parameters of the magnetic field environment include the magnetic field direction and the magnetic field intensity.
[0008] Further, the determination to stop generating the prepolymer is based on the comparison result that the NCO value is greater than or equal to a preset NCO value.
[0009] Furthermore, the process of determining whether the preparation process of the polyurethane composite material meets the standard based on the thermal conductivity coefficient includes: comparing the thermal conductivity with a preset thermal conductivity; Based on the comparison result that the thermal conductivity is less than the preset thermal conductivity, it is determined that the preparation process of the polyurethane composite material does not meet the standard.
[0010] Furthermore, the process of determining whether the arrangement direction of a single modified carbon nanotube meets the standard based on the inclination angle of the single modified carbon nanotube includes: comparing the tilt angle with a preset tilt angle; Determining that the arrangement direction of the single modified carbon nanotube does not meet the standard based on the comparison result that the inclination angle is greater than the preset inclination angle; Based on the comparison result that the tilt angle is less than or equal to the preset tilt angle, it is determined that the arrangement direction of the single modified carbon nanotube meets the standard.
[0011] Furthermore, the process of determining whether the setting of the magnetic field environment meets the standard based on the quantity ratio includes: Comparing the quantity ratio with a preset quantity ratio; Determining that the setting of the magnetic field environment meets the standard based on a comparison result that the quantity ratio is greater than or equal to the preset quantity ratio; Based on the comparison result that the number ratio is less than the preset number ratio, it is determined that the setting of the magnetic field environment does not meet the standard.
[0012] Further, under the condition that the setting of the magnetic field environment meets the standard, the process of adjusting the aspect ratio based on the thermal conductivity difference includes: Subtracting the thermal conductivity from the preset thermal conductivity to obtain a thermal conductivity difference; comparing the thermal conductivity difference with a preset thermal conductivity difference; The adjustment coefficient of the aspect ratio is determined based on a comparison result of the thermal conductivity difference and the preset thermal conductivity difference.
[0013] Further, under the condition that the setting of the magnetic field environment does not meet the standard, the process of adjusting the setting parameters of the magnetic field environment based on the tilt angle difference includes: comparing the tilt angle difference with a preset tilt angle difference; Determining the direction of the magnetic field to be adjusted based on a comparison result that the tilt angle difference is less than or equal to the preset tilt angle difference; The adjustment of the magnetic field strength is determined based on a comparison result that the tilt angle difference is greater than the preset tilt angle difference.
[0014] Furthermore, the preset tilt angle difference is subtracted from the tilt angle difference to obtain a first difference percentage, and several adjustment methods are set for the magnetic field direction based on the first difference percentage, and each adjustment method has a different adjustment amplitude for the magnetic field direction.
[0015] Furthermore, the inclination angle difference is subtracted from the preset inclination angle difference to obtain a second difference percentage, and several adjustment methods are set for the magnetic field strength based on the second difference percentage, and the adjustment amplitude of the magnetic field strength of each adjustment method is positively correlated with the second difference percentage.
[0016] Furthermore, in the step S3, a thermally conductive filler may be added to react with the modified carbon nanotubes and the polyurethane dispersion to generate a polyurethane composite material with a high thermal conductivity.
[0017] Compared with the prior art, the invention has the following beneficial effects: the invention uses a strong acid mixture to modify the carbon nanotubes, introduces oxygen-containing functional groups on the surface of the carbon nanotubes, improves the hydrophilicity of the carbon nanotubes, and increases the reactivity of the carbon nanotubes with the polyurethane molecular chain, thereby improving the dispersibility of the carbon nanotubes in the polyurethane emulsion; applies a magnetic field during the reaction of the modified carbon nanotubes and the polyurethane dispersion, and uses the magnetic anisotropy of the modified carbon nanotubes to induce the modified carbon nanotubes to be oriented in the polyurethane dispersion, thereby forming an effective heat conduction channel, so that heat can be quickly transferred along the direction of the carbon nanotubes, and the scattering and reflection of heat in the composite material are reduced, thereby improving the thermal conductivity of the composite material; through the thermal conductivity of the polyurethane composite material with high thermal conductivity finally obtained, it is determined whether the preparation process of the composite material meets the standard, and a microscopic analysis is performed on the preparation process that does not meet the standard, and the arrangement of the modified carbon nanotubes in the composite material is obtained to determine whether the setting of the magnetic field environment is unqualified or the aspect ratio of the carbon nanotubes is unqualified, and targeted adjustments are made for the unqualified factors, thereby improving the monitoring accuracy of the preparation process of the polyurethane composite material and improving the preparation efficiency of the polyurethane composite material.
[0018] Furthermore, the present invention determines whether to stop the reaction of generating the prepolymer based on the NCO value. The NCO value is an important indicator for measuring the content of isocyanate groups in the prepolymer. As the NCO value increases, the hardness, strength, wear resistance and weather resistance of the polyurethane composite material will increase. An excessively high NCO value will cause the composite material to be too hard and brittle, with reduced wear resistance and weather resistance and poor processing performance. Therefore, the NCO value in the preparation process of the composite material is periodically detected to determine the time node for stopping the generation of the prepolymer, thereby improving the monitoring accuracy of the preparation process of the polyurethane composite material and improving the preparation efficiency of the polyurethane composite material.
[0019] Furthermore, the present invention determines whether the preparation process of the polyurethane composite material meets the standards based on the thermal conductivity coefficient, obtains a microscopic image of the polyurethane composite material for the preparation process that does not meet the standards, determines the arrangement of the modified carbon nanotubes, determines whether the arrangement direction of the carbon nanotubes meets the standards, and adjusts the magnetic field strength or magnetic field direction for the situation that the arrangement direction of the carbon nanotubes does not meet the standards. The greater the magnetic field strength, the better the directional arrangement effect of the modified carbon nanotubes. Too high a magnetic field strength may cause structural damage to the carbon nanotubes or produce other adverse effects. For the situation that the arrangement direction of the modified carbon nanotubes meets the standards, the aspect ratio of the carbon nanotubes is adjusted. The greater the aspect ratio, the better the thermal conductivity of the carbon nanotubes, thereby improving the monitoring accuracy of the preparation process of the polyurethane composite material and further improving the preparation efficiency of the polyurethane composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a step diagram of a method for preparing a polyurethane composite material with high thermal conductivity according to an embodiment of the present invention; Figure 2 A flow chart for determining to stop generating the prepolymer according to an embodiment of the present invention; Figure 3 A flow chart for determining whether the preparation process of the polyurethane composite material meets the standards according to an embodiment of the present invention; Figure 4 The present invention is a flowchart for determining whether the setting of the magnetic field environment meets the standard according to the embodiment of the present invention. DETAILED DESCRIPTION
[0021] In order to make the objects and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with embodiments; it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0022] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.
[0023] It should be noted that, in the description of the present invention, terms such as "up", "down", "left", "right", "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is merely for the convenience of description and does not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present invention.
[0024] In addition, it should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0025] See also Figure 1-4 As shown, Figure 1 This is a step diagram of a method for preparing a polyurethane composite material with high thermal conductivity according to an embodiment of the present invention; Figure 2 A flow chart for determining to stop generating the prepolymer according to an embodiment of the present invention; Figure 3 A flow chart for determining whether the preparation process of the polyurethane composite material meets the standards according to an embodiment of the present invention; Figure 4 The present invention is a flowchart for determining whether the setting of the magnetic field environment meets the standard according to the embodiment of the present invention.
[0026] An embodiment of the present invention provides a method for preparing a polyurethane composite material with high thermal conductivity, comprising: Step S1, ultrasonically dispersing the washed carbon nanotubes in a solvent to form a dispersion, adding a strong acid mixture to the dispersion for heating and reflux treatment, filtering after refluxing for a preset time to obtain a filtrate, treating the filtrate and drying it to obtain modified carbon nanotubes; Step S2, respectively adding the dehydrated polyol and isocyanate to a first reaction kettle, adding a first catalyst under nitrogen protection to generate a prepolymer, periodically detecting the NCO value to determine whether to stop generating the prepolymer, and adding a hydrophilic chain extender, a crosslinking agent and a stabilizer under the condition of stopping generating the prepolymer to generate a polyurethane dispersion; Step S3, adding the modified carbon nanotubes and the polyurethane dispersion into a second reactor in a preset ratio, placing the second reactor in a magnetic field environment after ultrasonic dispersion, and adding a second catalyst to generate a polyurethane composite material with a high thermal conductivity; Step S4, obtaining the thermal conductivity of the polyurethane composite material, determining whether the preparation process of the polyurethane composite material meets the standard based on the thermal conductivity, obtaining a microscopic distribution image of the modified carbon nanotubes based on the preparation process of the polyurethane composite material that does not meet the standard, determining whether the arrangement direction of a single modified carbon nanotube meets the standard based on the inclination angle of the single modified carbon nanotube, counting the number ratio of the modified carbon nanotubes whose arrangement direction meets the standard and determining whether the setting of the magnetic field environment meets the standard based on the number ratio, and, under the condition that the magnetic field environment meets the standard, adjusting the aspect ratio of the carbon nanotubes based on the thermal conductivity difference, and under the condition that the magnetic field environment does not meet the standard, adjusting the setting parameters of the magnetic field environment based on the inclination angle difference, wherein the setting parameters of the magnetic field environment include the magnetic field direction and the magnetic field intensity.
[0027] Specifically, the filtrate is treated by repeatedly washing the filtrate with deionized water until the filtrate is neutral to remove residual acid and impurities.
[0028] Specifically, the first reactor is a reactor used for reacting polyol and isocyanate, and the second reactor is a reactor used for reacting modified carbon nanotubes and the polyurethane dispersion.
[0029] Specifically, the carbon nanotubes include multi-walled carbon nanotubes or single-walled carbon nanotubes, which are not specifically limited; the strong acid mixture is a mixture of concentrated sulfuric acid and concentrated nitric acid in a ratio of 3:1.
[0030] Specifically, the preset duration of the reflow processing is in the range of [8h, 15h], and 12h is preferred in the embodiment of the present invention.
[0031] Specifically, the polyol in the embodiment of the present invention is an oligomer polyol such as polyester polyol or polyether polyol, which is not specifically limited; the isocyanate is such as diphenylmethane diisocyanate or toluene diisocyanate, which is not specifically limited.
[0032] Specifically, the preset ratio is the mass ratio of the modified carbon nanotubes to the mass ratio of the polyurethane in the polyurethane dispersion, and the value range of the preset ratio is [0.05, 0.5], and 0.2 is preferred in the embodiment of the present invention.
[0033] Specifically, the first catalyst includes a tertiary amine catalyst, an organic metal compound catalyst and an inorganic salt catalyst, which are not specifically limited; the second catalyst includes an organic amine catalyst or an organic metal compound catalyst, which are not specifically limited.
[0034] Specifically, the NCO value is the mass of isocyanate (-NCO) groups contained in 100g of the sample, and the detection process of the NCO value is: Accurately weigh 5 g of the prepolymer mixture and place it in a conical flask; Use a pipette to add excess dibutylamine solution, shake to mix the liquid in the bottle evenly, and leave it at room temperature for 20-30 minutes to ensure that the prepolymer mixture and dibutylamine react fully; Add 40-50 ml of isopropanol and several drops of bromocresol green as an indicator, then titrate the remaining dibutylamine with a 0.5 mol / L standard hydrochloric acid solution. The titration is completed when the color of the solution changes from blue to yellow. Record the volume of the first standard hydrochloric acid solution consumed. Perform a blank experiment and record the volume of the second standard hydrochloric acid solution consumed; The NCO value is calculated according to the following formula:
[0035] Wherein, w represents the mass fraction of -NCO, V0 represents the volume of standard hydrochloric acid solution consumed in blank titration, V1 represents the volume of standard hydrochloric acid solution consumed in sample titration, c is the concentration of hydrochloric acid solution, m is the sample mass, and 42 is the molar mass of -NCO.
[0036] Specifically, the hydrophilic chain extender includes anionic, cationic and nonionic types, which are not specifically limited; the cross-linking agent includes polyols and amines, which are not specifically limited; the stabilizer includes free radical chain blocking agents and ultraviolet absorbers, which are not specifically limited.
[0037] Specifically, the thermal conductivity of polyurethane composite materials is tested using the heat flow meter method, and the specific process is as follows: The polyurethane composite material sample is processed into a cube with a side length of 5 cm, and a heat flow meter such as a TC2100 heat flow meter thermal conductivity meter is selected, and the specific details are not limited; The sample is clamped between two heat flux sensors, and the heating unit is started to apply a constant heat flux to the sample; Under the condition that the heat flux density and temperature no longer change significantly, record the output value of the heat flux sensor; Calculate the heat flux density passing through the sample according to the output value of the heat flux sensor and the calibration coefficient; The thermal conductivity is calculated using Fourier's law of heat conduction based on the heat flux, sample thickness and temperature gradient.
[0038] Specifically, the tilt angle is the angle between the arrangement direction of a single carbon nanotube and a standard direction, and the standard direction is a direction in which the arrangement direction of a single carbon nanotube has no tilt and completely meets the design requirements.
[0039] Specifically, the magnetic field strength is provided by a magnetic field source, which includes an electromagnet, a permanent magnet and a superconducting magnet, without specific limitation.
[0040] Specifically, the microscopic distribution image of the modified carbon nanotubes is obtained using a scanning electron microscope, and the model and parameters of the scanning electron microscope are not specifically limited.
[0041] Specifically, the present invention uses a strong acid mixture to modify the carbon nanotubes, introduces oxygen-containing functional groups on the surface of the carbon nanotubes, and improves the hydrophilicity of the carbon nanotubes while increasing the reactivity of the carbon nanotubes with polyurethane molecular chains, thereby improving the dispersibility of the carbon nanotubes in the polyurethane emulsion; by applying a magnetic field during the reaction of the modified carbon nanotubes and the polyurethane dispersion, the magnetic anisotropy of the modified carbon nanotubes is used to induce the modified carbon nanotubes to be oriented in the polyurethane dispersion, thereby forming an effective heat conduction channel, so that heat can be quickly transferred along the direction of the carbon nanotubes, and the scattering and reflection of heat in the composite material are reduced, thereby improving the thermal conductivity of the composite material; through the thermal conductivity of the polyurethane composite material with high thermal conductivity finally obtained, it is determined whether the preparation process of the composite material meets the standard, and a microscopic analysis is performed on the preparation process that does not meet the standard, and the arrangement of the modified carbon nanotubes in the composite material is obtained to determine whether the setting of the magnetic field environment is unqualified or the aspect ratio of the carbon nanotubes is unqualified, and targeted adjustments are made for the unqualified factors, thereby improving the monitoring accuracy of the preparation process of the polyurethane composite material and improving the preparation efficiency of the polyurethane composite material.
[0042] Specifically, the determining to stop generating the prepolymer based on the comparison result that the NCO value is greater than or equal to a preset NCO value; The process further determines to continue to generate the prepolymer based on the comparison result that the NCO value is less than the preset NCO value.
[0043] Specifically, the preset NCO value is determined according to the performance design requirements of the polyurethane composite material.
[0044] The present invention determines whether to stop the reaction of generating a prepolymer based on an NCO value. The NCO value is an important indicator for measuring the content of isocyanate groups in the prepolymer. As the NCO value increases, the hardness, strength, wear resistance and weather resistance of the polyurethane composite material increase. An excessively high NCO value will cause the composite material to be too hard and brittle, and the wear resistance and weather resistance will decrease, and the processing performance will deteriorate. Therefore, the NCO value in the preparation process of the composite material is periodically detected to determine the time node for stopping the generation of the prepolymer, thereby improving the monitoring accuracy of the preparation process of the polyurethane composite material and improving the preparation efficiency of the polyurethane composite material.
[0045] Specifically, the process of determining whether the preparation process of the polyurethane composite material meets the standard based on the thermal conductivity includes: comparing the thermal conductivity with a preset thermal conductivity; Determining that the preparation process of the polyurethane composite material does not meet the standard based on the comparison result that the thermal conductivity is less than the preset thermal conductivity; Based on the comparison result that the thermal conductivity is greater than or equal to the preset thermal conductivity, it is determined that the preparation process of the polyurethane composite material meets the standard.
[0046] Specifically, the preset thermal conductivity coefficient is set in the range of [0.2 W / (m·K), 1.2 W / (m·K)], and 0.5 W / (m·K) is preferred in the embodiment of the present invention.
[0047] Specifically, the greater the thermal conductivity, the better the thermal conductivity of the polyurethane composite material.
[0048] Specifically, the process of determining whether the arrangement direction of a single modified carbon nanotube meets the standard based on the inclination angle of the single modified carbon nanotube includes: comparing the tilt angle with a preset tilt angle; Determining that the arrangement direction of the single modified carbon nanotube does not meet the standard based on the comparison result that the inclination angle is greater than the preset inclination angle; Based on the comparison result that the tilt angle is less than or equal to the preset tilt angle, it is determined that the arrangement direction of the single modified carbon nanotube meets the standard.
[0049] Specifically, the value range of the preset tilt angle is set to (0°, 20°], and 10° is preferred in the embodiment of the present invention.
[0050] Specifically, the smaller the tilt angle, the more standardized the directional arrangement of the modified carbon nanotubes and the higher the thermal conductivity of the composite material.
[0051] Specifically, the process of determining whether the setting of the magnetic field environment meets the standard based on the quantity ratio includes: Comparing the quantity ratio with a preset quantity ratio; Determining that the setting of the magnetic field environment meets the standard based on a comparison result that the quantity ratio is greater than or equal to the preset quantity ratio; Based on the comparison result that the number ratio is less than the preset number ratio, it is determined that the setting of the magnetic field environment does not meet the standard.
[0052] Specifically, the value range of the preset quantity ratio is set to [60%, 100%], and 80% is preferred in the embodiment of the present invention.
[0053] Specifically, under the condition that the setting of the magnetic field environment meets the standard, the process of adjusting the aspect ratio based on the thermal conductivity difference includes: Subtracting the thermal conductivity from the preset thermal conductivity to obtain a thermal conductivity difference; comparing the thermal conductivity difference with a preset thermal conductivity difference; Determining to use a first adjustment coefficient to adjust the aspect ratio based on a comparison result that the thermal conductivity difference is greater than the preset thermal conductivity difference; Based on the comparison result that the thermal conductivity difference is less than or equal to the preset thermal conductivity difference, it is determined that the second adjustment coefficient is used to adjust the aspect ratio.
[0054] Specifically, the preset thermal conductivity difference value range is set to [0.02 W / (m·K), 0.2 W / (m·K)], and 0.15 W / (m·K) is preferred in the embodiment of the present invention.
[0055] Specifically, the value range of the first adjustment coefficient is set to [1.3, 1.5], and 1.4 is preferably selected in the embodiment of the present invention; the value range of the second adjustment coefficient is set to [1.01, 1.29], and 1.2 is preferably selected in the embodiment of the present invention.
[0056] Specifically, under the condition that the setting of the magnetic field environment does not meet the standard, the process of adjusting the setting parameters of the magnetic field environment based on the tilt angle difference includes: comparing the tilt angle difference with a preset tilt angle difference; Determining the direction of the magnetic field to be adjusted based on a comparison result that the tilt angle difference is less than or equal to the preset tilt angle difference; The adjustment of the magnetic field strength is determined based on a comparison result that the tilt angle difference is greater than the preset tilt angle difference.
[0057] Specifically, the value range of the preset tilt angle difference is set to (0°, 10°], and 5° is preferred in the embodiment of the present invention.
[0058] Specifically, the preset tilt angle difference is subtracted from the tilt angle difference to obtain a first difference percentage, and several adjustment methods are set for the magnetic field direction based on the first difference percentage, and each adjustment method has a different adjustment amplitude for the magnetic field direction.
[0059] Specifically, if the first difference percentage is greater than a first preset difference percentage, it is determined to use a first angle adjustment coefficient to adjust the direction of the magnetic field; If the first difference percentage is less than or equal to the first preset difference percentage, it is determined to use the second angle adjustment coefficient to adjust the magnetic field direction.
[0060] Specifically, the adjustment of the direction of the magnetic field is controlled by adjusting the angle at which the magnetic flux lines pass through the second reactor. The smaller the angle, the closer the direction in which the magnetic flux lines pass through the second reactor is to the vertical direction of the second reactor. When the angle is 0°, the magnetic flux lines pass through the second reactor vertically. The smaller the angle at which the magnetic flux lines pass through the second reactor, the stronger the traction force on the modified carbon nanotubes. The adjustment direction of the magnetic field direction is in the opposite direction to the tilt angle.
[0061] Specifically, the value range of the first preset difference percentage is set to [4%, 8%], and 5% is preferred in the embodiment of the present invention; the value range of the first angle adjustment coefficient is set to [0.8, 0.89], and 0.85 is preferred in the embodiment of the present invention; the value range of the second angle adjustment coefficient is set to [0.9, 0.99], and 0.95 is preferred in the embodiment of the present invention.
[0062] Specifically, the tilt angle difference is subtracted from the preset tilt angle difference to obtain a second difference percentage, and several adjustment methods are set for the magnetic field strength based on the second difference percentage, and the adjustment amplitude of the magnetic field strength in each adjustment method is positively correlated with the second difference percentage.
[0063] Specifically, it can be understood that the adjustment range of the magnetic field strength by each adjustment method is positively correlated with the second difference percentage, and the larger the second difference percentage is, the larger the adjustment range of the magnetic field strength is.
[0064] Specifically, in step S3, a thermally conductive filler may be added to react with the modified carbon nanotubes and the polyurethane dispersion to generate a polyurethane composite material with a high thermal conductivity.
[0065] Specifically, the thermally conductive filler includes metal fillers such as copper, aluminum, and silver, and ceramic fillers such as aluminum oxide, boron nitride, and silicon carbide, without limitation.
[0066] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.
Claims
1. A method for preparing a polyurethane composite material with high thermal conductivity, characterized in that: include: Step S1, ultrasonically dispersing the washed carbon nanotubes in a solvent to form a dispersion, adding a strong acid mixture to the dispersion for heating and reflux treatment, filtering after refluxing for a preset time to obtain a filtrate, treating the filtrate and drying it to obtain modified carbon nanotubes; Step S2, respectively adding the dehydrated polyol and isocyanate to a first reaction kettle, adding a first catalyst under nitrogen protection to generate a prepolymer, periodically detecting the NCO value to determine whether to stop generating the prepolymer, and adding a hydrophilic chain extender, a crosslinking agent and a stabilizer under the condition of stopping generating the prepolymer to generate a polyurethane dispersion; Step S3, adding the modified carbon nanotubes and the polyurethane dispersion into a second reactor in a preset ratio, placing the second reactor in a magnetic field environment after ultrasonic dispersion, and adding a second catalyst to generate a polyurethane composite material with a high thermal conductivity; Step S4, obtaining the thermal conductivity of the polyurethane composite material, determining whether the preparation process of the polyurethane composite material meets the standard based on the thermal conductivity, obtaining a microscopic distribution image of the modified carbon nanotubes based on the preparation process of the polyurethane composite material that does not meet the standard, determining whether the arrangement direction of a single modified carbon nanotube meets the standard based on the inclination angle of the single modified carbon nanotube, counting the number ratio of the modified carbon nanotubes whose arrangement direction meets the standard and determining whether the setting of the magnetic field environment meets the standard based on the number ratio, and, under the condition that the magnetic field environment meets the standard, adjusting the aspect ratio of the carbon nanotubes based on the thermal conductivity difference, and under the condition that the magnetic field environment does not meet the standard, adjusting the setting parameters of the magnetic field environment based on the inclination angle difference, wherein the setting parameters of the magnetic field environment include the magnetic field direction and the magnetic field intensity.
2. The method for preparing a polyurethane composite material with high thermal conductivity according to claim 1, characterized in that: The stopping of the production of the prepolymer is determined based on a comparison result that the NCO value is greater than or equal to a preset NCO value.
3. The method for preparing a polyurethane composite material with high thermal conductivity according to claim 2, characterized in that: The process of determining whether the preparation process of the polyurethane composite material meets the standard based on the thermal conductivity includes: comparing the thermal conductivity with a preset thermal conductivity; Based on the comparison result that the thermal conductivity is less than the preset thermal conductivity, it is determined that the preparation process of the polyurethane composite material does not meet the standard.
4. The method for preparing a polyurethane composite material with high thermal conductivity according to claim 3, characterized in that: The process of determining whether the arrangement direction of a single modified carbon nanotube meets the standard based on the inclination angle of the single modified carbon nanotube comprises: comparing the tilt angle with a preset tilt angle; Determining that the arrangement direction of the single modified carbon nanotube does not meet the standard based on the comparison result that the inclination angle is greater than the preset inclination angle; Based on the comparison result that the tilt angle is less than or equal to the preset tilt angle, it is determined that the arrangement direction of the single modified carbon nanotube meets the standard.
5. The method for preparing a polyurethane composite material with high thermal conductivity according to claim 4, characterized in that: The process of determining whether the setting of the magnetic field environment meets the standard based on the quantity ratio includes: Comparing the quantity ratio with a preset quantity ratio; Determining that the setting of the magnetic field environment meets the standard based on a comparison result that the quantity ratio is greater than or equal to the preset quantity ratio; Based on the comparison result that the number ratio is less than the preset number ratio, it is determined that the setting of the magnetic field environment does not meet the standard.
6. The method for preparing a polyurethane composite material with high thermal conductivity according to claim 5, characterized in that: Under the condition that the setting of the magnetic field environment meets the standard, the process of adjusting the aspect ratio based on the thermal conductivity difference includes: Subtracting the thermal conductivity from the preset thermal conductivity to obtain a thermal conductivity difference; comparing the thermal conductivity difference with a preset thermal conductivity difference; The adjustment coefficient of the aspect ratio is determined based on a comparison result of the thermal conductivity difference and the preset thermal conductivity difference.
7. The method for preparing a polyurethane composite material with high thermal conductivity according to claim 5, characterized in that: Under the condition that the setting of the magnetic field environment does not meet the standard, the process of adjusting the setting parameters of the magnetic field environment based on the tilt angle difference includes: comparing the tilt angle difference with a preset tilt angle difference; Determining the direction of the magnetic field to be adjusted based on a comparison result that the tilt angle difference is less than or equal to the preset tilt angle difference; The adjustment of the magnetic field strength is determined based on a comparison result that the tilt angle difference is greater than the preset tilt angle difference.
8. The method for preparing a polyurethane composite material with high thermal conductivity according to claim 7, characterized in that: The preset tilt angle difference is subtracted from the tilt angle difference to obtain a first difference percentage, and several adjustment methods are set for the magnetic field direction based on the first difference percentage, and each adjustment method has a different adjustment amplitude for the magnetic field direction.
9. The method for preparing a polyurethane composite material with high thermal conductivity according to claim 7, characterized in that: The inclination angle difference is subtracted from the preset inclination angle difference to obtain a second difference percentage, and several adjustment methods are set for the magnetic field strength based on the second difference percentage, and the adjustment amplitude of the magnetic field strength in each adjustment method is positively correlated with the second difference percentage.
10. The method for preparing a polyurethane composite material with high thermal conductivity according to claim 9, characterized in that: In the step S3, a thermally conductive filler may be added to react with the modified carbon nanotubes and the polyurethane dispersion to generate a polyurethane composite material with a high thermal conductivity.
Citation Information
Patent Citations
Multifunctional light nano-composite foam and preparation method and application thereof
CN106220821A
Carbon nanotubes comprising hydroxy groups, method for the production thereof and polyurethane polymers comprising said carbon nanotubes
US20120029162A1
High-performance thermal interface films and methods thereof
WO2012111837A1