Polyurethane wet-process hydrolysis-resistant resin for soft non-fogging mirror leather and preparation method of polyurethane wet-process hydrolysis-resistant resin
By using polyurethane wet hydrolysis-resistant resin in the wet mirror leather resin and combining specific polyether polyols and additives, the problem of insufficient surface mist and peel strength of the wet mirror leather resin in the prior art is solved, and the problem of insufficient surface mist and peel strength of the resin for wet mirror leather is achieved. The high washing performance and 5 years of hydrolysis resistance have improved the added value and application range of the product.
Patent Information
- Application Number
- CN202410930685.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-15
AI Technical Summary
The existing soft 2-year hydrolysis resistance and 5-year hydrolysis resistance wet mirror leather resin is prone to surface mist after processing, insufficient peeling strength, poor tightness and elasticity, and it is difficult to take into account both 5-year hydrolysis resistance and good water washing performance. Limits the added value of the product and application development.
Using a polyurethane wet-resistant hydrolysis resin for soft, non-fogging mirror leather, the polyether polyol with mixed structure of polytetrahydrofuran, polypropylene oxide and ethylene oxide is used in the formulation to combine small molecule alcohols and specific Additives, such as end-hydroxyalkyl polysiloxane, adjust the film forming, washing and tightness of the resin, and ensure the viscosity and solid content of the resin through specific process steps and temperature control.
It significantly improves the surface gloss, flesh solid feeling, washing performance and peel strength of synthetic leather, extends the hydrolysis resistance, reduces the risk of fogging, expands the application range of the product and increases added value.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane materials, and in particular relates to a polyurethane wet-process hydrolysis-resistant resin for soft, non-fogging mirror leather, and a preparation method and application thereof. Background Art
[0002] Wet-process hydrolysis-resistant resin for mirror leather means that the prepared hydrolysis-resistant resin is first applied to the mirror high-F cloth, and then put into water through a series of processes such as solidification, washing, and drying with a scraper of fixed thickness to form a wet-process base, and then a layer of dry-process mirror resin is attached to the surface of the wet-process base to form a mirror-like hydrolysis-resistant synthetic leather.
[0003] Currently, there are two types of soft, 2-year hydrolysis-resistant wet-process mirror leather resins and five-year hydrolysis-resistant wet-process mirror leather resins on the market. To achieve better washability, the soft, 2-year hydrolysis-resistant wet-process mirror leather resin is formulated by adding a certain amount of polyester polyol to the polyether polyol. This is then processed into synthetic leather using a wet process. However, this method has the disadvantage that the processed mirror leather may not achieve the desired five-year hydrolysis resistance, exhibit insufficient peel strength, and experience surface fogging, which can extend beyond the five-year hydrolysis resistance period. Regarding the soft 5-year hydrolysis-resistant wet-process mirror leather resin, in order to achieve better water washing performance, the high molecular weight polypropylene oxide structure polyether polyol and the moderate molecular weight polytetrahydrofuran structure polyether polyol are combined in the design formula to improve the performance, and the synthetic leather is produced by the wet process for mirror leather; the disadvantage of this method is that the back of the synthetic leather after processing is prone to rough creases, a tight and poor elasticity, and a foggy surface; the soft 2-year hydrolysis-resistant mirror leather resin and the soft 5-year hydrolysis-resistant mirror leather resin currently sold on the market cannot simultaneously achieve 5-year hydrolysis resistance and good water washing performance, so that the back-end application development of mirror leather resins in various styles has encountered bottlenecks, making it difficult to increase the added value of products on the market.
[0004] Therefore, it is very necessary to develop a soft, non-fogging, mirror leather polyurethane wet-process hydrolysis-resistant resin. Summary of the Invention
[0005] In view of the problems that the existing 5-year hydrolysis-resistant mirror synthetic leather is prone to surface fogging, poor texture and elasticity, and the risk of fogging of the mirror synthetic leather increases due to insufficient water washing, and it is difficult to increase the added value of back-end application products, the present invention provides a soft, non-fogging polyurethane wet-process hydrolysis-resistant resin for mirror leather, as well as its preparation method and application.
[0006] In a first aspect, the present invention provides a polyurethane wet-process hydrolysis-resistant resin for soft, non-fogging mirror leather, the raw materials for its preparation comprising the following components in parts by weight:
[0007] 0.001-0.003 parts of inorganic acid;
[0008] 175-235 parts of polyether polyol;
[0009] 66-88 parts of isocyanate;
[0010] 17-23 parts of small molecule alcohol;
[0011] 9-12 parts of additives;
[0012] 630-839 parts of solvent.
[0013] Preferably, the inorganic acid is concentrated phosphoric acid. In the synthesis of leather resin, a phosphoric acid solution with a concentration of 80%-90% is usually referred to as "concentrated phosphoric acid". The concentrated phosphoric acid herein can be any value within the above concentration range.
[0014] Preferably, the polyether polyol includes: a polyether polyol with a polytetrahydrofuran structure (denoted as PE-1), a polyether polyol with a mixed structure of polytetrahydrofuran and ethylene oxide (denoted as PE-2), and a polyether polyol with a mixed structure of polypropylene oxide and ethylene oxide (denoted as PE-3), wherein the molar ratio of the tetrahydrofuran unit to the ethylene oxide unit in PE-2 is 4.5-4.8:0.1-0.2, and the molar ratio of the propylene oxide unit to the ethylene oxide unit in PE-3 is 2.8-3:1.8-2.
[0015] Preferably, the molecular weight range of PE-1 and PE-2 is a number average molecular weight of 1000-2200; the molecular weight range of PE-3 is a number average molecular weight of 3800-4200.
[0016] Preferably, the molecular weight of PE-1 is 1000; the molecular weight of PE-2 is 2000; and the molecular weight of PE-3 is 4000.
[0017] Preferably, the isocyanate is one or more of diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), and dicyclohexylmethane diisocyanate (HMDI), preferably diphenylmethane diisocyanate (MDI).
[0018] Preferably, the small molecule alcohol is one or more of 1,3-butanediol (1,3-BG), 2-methylpropanediol, and dodecanediol, as a chain extender, preferably 1,3-butanediol.
[0019] Preferably, the solvent is N,N-dimethylformamide (DMF), and the auxiliary agent is one or more of a water-assisting agent, a stabilizer, a capping agent, and a hindered phenol antioxidant.
[0020] Preferably, the water-assisting agent is a terminal hydroxyalkyl polysiloxane, which can be a commercially available product.
[0021] Preferably, the stabilizer is benzoic acid.
[0022] Preferably, the capping agent is methanol.
[0023] In a second aspect, the present invention further provides a method for preparing the above-mentioned soft, non-fogging, mirror leather polyurethane wet-process hydrolysis-resistant resin, comprising the following steps:
[0024] (1) PE-1, PE-2 and PE-3 in the polyether polyol, a small molecule alcohol, a hindered phenol antioxidant, an inorganic acid, and a portion of the solvent are mixed and subjected to a heating treatment;
[0025] (2) adding a portion of isocyanate to the mixture treated in step (1) and treating at a constant temperature;
[0026] (3) adding the remaining isocyanate to the mixture after treatment in step (2) to carry out reaction, and maintaining the R value at 0.9-1.1, adding the remaining solvent until the viscosity of the reaction liquid is 20-26 Pas / 25 degrees and the solid content of the reaction liquid is 30%-31%, and then adding the blocking agent, stirring and cooling; (4) adding a stabilizer and a water-aiding detergent to the mixture after treatment in step (3) and stirring to obtain a polyurethane wet-process hydrolysis-resistant resin.
[0027] Preferably, the preparation of the polyurethane wet-process hydrolysis-resistant resin is completed in a reactor.
[0028] Preferably, in step (1), the temperature is raised to 40°C-50°C, and after the temperature is raised, the mixture is stirred at the constant temperature for 20-40 minutes. Preferably, based on the total mass of the solvent being 100%, the mass percentage of the solvent in step (1) is 55%-60%.
[0029] Preferably, in step (2), the constant temperature treatment condition is stirring at 70° C.-75° C. for 1-3 hours; and the amount of isocyanate added is 90%-95% (mass percentage) of the total amount of isocyanate.
[0030] Preferably, in step (3), the temperature is controlled at 70° C.-75° C. during the addition of the remaining isocyanate.
[0031] In a third aspect, the present invention also provides a synthetic leather, which is prepared using the above-mentioned polyurethane wet-process hydrolysis-resistant resin for soft non-fogging mirror leather, or prepared using a resin prepared by the above-mentioned preparation method of the polyurethane wet-process hydrolysis-resistant resin for soft non-fogging mirror leather.
[0032] Beneficial effects: (1) In the preparation of the polyurethane wet-process hydrolysis-resistant resin in the present invention, different polyether polyols PE1, PE2 and PE3 are selected in combination to improve the film-forming property and firmness and thickness of the synthetic leather base surface; the water washability and thickness of the resin are improved, which is easier to coordinate the changes in the water washability of the main body than the selection of a single-structure polyether polyol; the resin solidification speed is increased by using a small molecule alcohol as a chain extender to make the resin more uniform while ensuring the improvement of the firm feel, and the modulus, solidification speed and gloss of the resin are increased by increasing the amount of the chain extender, which is easier to adjust than using a weakly crystalline chain extender; in the selection of auxiliary agents, an auxiliary agent that is conducive to uniform solidification, water washability and improves the gloss of synthetic leather is selected, which significantly improves the surface gloss and firmness of the synthetic leather.
[0033] (2) In the preparation of the polyurethane wet-process hydrolysis-resistant resin of the present invention, by adjusting the ratio of different polyether polyols and combining them with a chain extender with strong crystallinity, a terminal hydroxyalkyl polysiloxane auxiliary agent, etc., the solidification speed, modulus, compactness, and water washability of the resin are significantly improved, so that when preparing the resin for mirror leather, it is possible to ensure good water washability combined with compactness and fine creases, thereby widening the application range of the rear end leather and increasing the added value.
[0034] (3) In the preparation of the polyurethane wet-process hydrolysis-resistant resin of the present invention, the water-washing performance of the resin is significantly improved by using polyether polyol PE-2, which plays a key role in the preparation of the polyurethane hydrolysis-resistant resin for mirror leather.
[0035] (4) In the preparation of the polyurethane wet-process hydrolysis-resistant resin of the present invention, by selecting a chain extender with strong crystallinity and combining it with a special structure polyether polyol PE-3 (a polyether polyol with a mixed structure of polypropylene oxide and ethylene oxide), good peel strength and firmness with fine creases can be ensured, while also ensuring 5-year hydrolysis resistance.
[0036] (5) In the preparation of the polyurethane wet-process hydrolysis-resistant resin of the present invention, the water-washing performance and the leveling property of the resin are improved by selecting a terminal hydroxyalkyl polysiloxane auxiliary agent (the terminal hydroxyalkyl polysiloxane contains hydroxyl groups and has a low molecular weight). The auxiliary agent is added at the end (a trace amount of isocyanate is contained at the end of the main reaction). The two can react and connect to increase the molecular weight of the water-washing auxiliary agent, thereby ensuring that the risk of fogging is significantly reduced. DETAILED DESCRIPTION
[0037] The present invention will now be further described in detail by way of examples, but the present invention is not limited to the examples.
[0038] The raw materials used in the examples of the present invention and the comparative examples are as follows:
[0039] PE-1 (polytetramethylene glycol polyol): molecular weight 1000 (Hyosung Group (Jiaxing) Co., Ltd., model: PTMG-2000);
[0040] PE-17 (polytetramethylene oxide-based polyether polyol): molecular weight 2000 (Hyosung Group (Jiaxing) Co., Ltd., model: PTMG-1000);
[0041] PE-2 (polyether polyol with a mixed structure of polytetrahydrofuran and ethylene oxide): molecular weight 2000 (BASF, Caojing, Shanghai, model: PTMG-2002, in which the molar ratio of tetrahydrofuran units to ethylene oxide units is approximately 4.8:0.2;
[0042] PE-3 (polyether polyol with a mixed structure of polypropylene oxide and ethylene oxide): molecular weight 4000 (Shandong Bluestar Dongda Co., Ltd., model: ED-28), in which the molar ratio of propylene oxide units to ethylene oxide units is approximately 3:2;
[0043] PE-4 (polypropylene oxide structured polyether polyol): molecular weight 4000 (Shandong Bluestar Dongda Co., Ltd., model: DP-4000D);
[0044] Hindered phenol antioxidant: ROX-13TP (Double Bond Chemical Co., Ltd., Taiwan, China, model: antioxidant 1330);
[0045] Water-assisting detergent terminal hydroxyalkyl polysiloxane: XP-555 (Shanghai Tiger Polymer Technology Co., Ltd., model: Tech-2140).
[0046] The raw materials used in the present invention are all commercially available commodities.
[0047] Example 1
[0048] A polyurethane wet-process hydrolysis-resistant resin for soft, non-fogging mirror leather, the raw materials for its preparation comprising the following components:
[0049] PE-1: 70g, PE-2: 35g, PE-3: 70g, hindered phenol antioxidant ROX-13TP: 0.2g, concentrated phosphoric acid: 0.002g, 1,3-butanediol: 18g, DMF: 630g, MDI: 75g, methanol: 0.75g, benzoic acid: 0.75g, terminal hydroxyalkyl polysiloxane XP-555: 9g.
[0050] The preparation method of the above-mentioned polyurethane wet-process hydrolysis-resistant resin is as follows.
[0051] (1) Add PE-1, PE-2, PE-3, 1,3-butanediol, hindered phenolic antioxidant ROX-13TP, concentrated phosphoric acid, and DMF (57% by mass) to a reactor according to the above mass, heat to 40°C, maintain constant temperature, and stir for 30 minutes;
[0052] (2) adding 92% of the total amount of MDI to the mixture treated in step (1), and stirring at 70° C. for 2 hours;
[0053] (3) Add the remaining 8% of MDI to the mixture after treatment in step (2) as appropriate and keep the R value at 1, and maintain the temperature at 70°C; add the remaining 43% of DMF until the viscosity of the reaction liquid reaches the theoretical viscosity of 26pas / 25 degrees set in the instruction table, and the solid content is 30%, add methanol capping agent, stir for 30 minutes, and cool to 60°C;
[0054] (4) Add benzoic acid and terminal hydroxyalkyl polysiloxane XP-555 to the mixture after treatment in step (3), and stir thoroughly for 1.5 hours to obtain a polyurethane wet-process hydrolysis-resistant resin.
[0055] Example 2
[0056] A polyurethane wet-process hydrolysis-resistant resin for soft, non-fogging mirror leather, the raw materials for its preparation comprising the following components:
[0057] PE-1: 70g, PE-2: 70g, PE-3: 35g, hindered phenol antioxidant ROX-13TP: 0.2g, concentrated phosphoric acid: 0.002g, 1,3-butanediol: 18g, DMF: 630g, MDI: 75g, methanol: 0.75g, benzoic acid: 0.75g, terminal hydroxyalkyl polysiloxane XP-555: 9g.
[0058] The preparation method of the above-mentioned polyurethane wet-process hydrolysis-resistant resin is as follows.
[0059] (1) Add PE-1, PE-2, PE-3, 1,3-butanediol, hindered phenolic antioxidant ROX-13TP, concentrated phosphoric acid, and DMF (57% by mass) to a reactor according to the above mass, heat to 40°C, maintain constant temperature, and stir for 30 minutes;
[0060] (2) adding 92% of the total amount of MDI to the mixture treated in step (1), and stirring at 70° C. for 2 hours;
[0061] (3) Add the remaining 8% of MDI to the mixture after treatment in step (2) as appropriate and keep the R value at 1, and maintain the temperature at 70°C; add the remaining 43% of DMF until the viscosity of the reaction liquid reaches the theoretical viscosity of 26pas / 25 degrees set in the instruction table, and the solid content is 30%, add methanol capping agent, stir for 30 minutes, and cool to 60°C;
[0062] (4) Add benzoic acid and terminal hydroxyalkyl polysiloxane XP-555 to the mixture after treatment in step (3), and stir thoroughly for 1.5 hours to obtain a polyurethane wet-process hydrolysis-resistant resin.
[0063] Example 3
[0064] A polyurethane wet-process hydrolysis-resistant resin for soft, non-fogging mirror leather, the raw materials for its preparation comprising the following components:
[0065] PE-1: 70g, PE-2: 35g, PE-4: 70g, hindered phenol antioxidant ROX-13TP: 0.2g, concentrated phosphoric acid: 0.002g, 1,3-butanediol: 18g, DMF: 630g, MDI: 75g, methanol: 0.75g, benzoic acid: 0.75g, terminal hydroxyalkyl polysiloxane XP-555: 9g.
[0066] The preparation method of the above-mentioned polyurethane wet-process hydrolysis-resistant resin is as follows.
[0067] (1) Add PE-1, PE-2, PE-4, 1,3-butanediol, hindered phenolic antioxidant ROX-13TP, concentrated phosphoric acid, and 57% (mass percentage) of DMF to the reactor according to the above mass, heat to 40°C, maintain constant temperature, and stir for 30 minutes;
[0068] (2) adding 92% of the total amount of MDI to the mixture treated in step (1), and stirring at 70° C. for 2 hours;
[0069] (3) Add the remaining 8% of MDI to the mixture after treatment in step (2) as appropriate and keep the R value at 1, and maintain the temperature at 70°C; add the remaining 43% of DMF until the viscosity of the reaction liquid reaches the theoretical viscosity of 26pas / 25 degrees set in the instruction table, and the solid content is 30%, add methanol capping agent, stir for 30 minutes, and cool to 60°C;
[0070] (4) Add benzoic acid and terminal hydroxyalkyl polysiloxane XP-555 to the mixture after treatment in step (3), and stir thoroughly for 1.5 hours to obtain a polyurethane wet-process hydrolysis-resistant resin.
[0071] Comparative Example 1
[0072] The preparation process is basically the same as that of Example 1, except that 12.4 g of ethylene glycol (EG) is used as the chain extender instead of 18 g of 1,3-butanediol.
[0073] Comparative Example 2
[0074] The preparation process is basically the same as that of Example 1, except that 21.2 g of diethylene glycol (DEG) is used as the chain extender instead of 18 g of 1,3-butanediol.
[0075] Comparative Example 3
[0076] The preparation process is basically the same as that of Example 1, except that a polyether polyol (PE-4) with a 4000 molecular weight polypropylene oxide structure is used to replace part of the 4000 molecular weight polyether polyol (PE-3).
[0077] Comparative Example 4
[0078] The preparation process is basically the same as that of Example 1, except that a polyether polyol with a polytetrahydrofuran structure having a molecular weight of 2000 (denoted as PE-17) is used instead of a polyether polyol with a molecular weight of 1000 (PE-1).
[0079] The raw materials and contents of the polyurethane wet-process hydrolysis-resistant resins of Examples 1-3 and Comparative Examples 1-4 are shown in Table 1, unit: g.
[0080] Table 1
[0081]
[0082] The polyurethane wet process hydrolysis resistant resins of Examples 1-3 and Comparative Examples 1-4 were prepared into mirror synthetic leather according to the following steps: 100 g of the synthesized polyurethane resin was added to a plastic bottle, 65 g of calcium carbonate, 1 g of oily special black paste and 65 g of solvent DMF were added thereto, and the mixture was heated at 3000 r·min. -1 The mixture is uniformly dispersed at a high speed under a stirring speed of , and then allowed to stand for degassing for standby use. The leather base cloth is soaked in a 20% DMF aqueous solution to remove impurities on its surface, and then the water is pressed with a water press, and then ironed with an iron until it is half dry, and then a 0.2mm thick feeler gauge is placed on the back of the base cloth. A small amount of the slurry to be used is poured on the front of the mirror high F cloth and scraped on it, and then placed in water for sufficient solidification, and then washed and dried to make a wet base cloth, and then pasted with a 15-thread thick dry mirror fabric to obtain the mirror synthetic leather of Examples 1-3 and the mirror synthetic leather of Comparative Examples 1-4.
[0083] The following performance tests were performed on the mirror synthetic leathers of Examples 1-3 and Comparative Examples 1-4, respectively, according to the test evaluation standards:
[0084] Creases: If the creases after applying dry mirror resin to the wet bass are fine, it is good; if there are thick creases, it is poor.
[0085] Thickness: When the resin coating is spread according to 100 lines of a fixed caliper, a thickness of 0.3 mm or more is considered excellent, and less than 0.1 mm is considered poor.
[0086] Peel strength: After drying at 110°C, the peel strength reaches 3.5 kg, which is excellent; if it does not reach 3.5 kg, it is poor.
[0087] Feel: If the firmness and rebound are good after drying at 110℃, it is excellent; if the firmness and rebound are not good, it is poor.
[0088] 5-year hydrolysis resistance: After soaking in 10% NaOH aqueous solution for 24 hours, the NaOH is washed off and dried. If the peel strength remains unchanged before and after soaking, it is excellent; if the peel strength decreases significantly before and after soaking, it is poor.
[0089] Water washing: If the surface is smooth after 15 times of squeezing with water washing roller, it is excellent; if the surface is uneven, it is poor.
[0090] Fogging: After dry-process mirror resin veneer veneer, if no layer of white frost is observed in a high-temperature, high-humidity environment for 6 months, it is considered excellent; if a layer of white frost is observed, it is considered poor. The results are shown in Table 2.
[0091] Table 2
[0092]
[0093] As shown in Table 2, Example 1 has good crease fineness, moderate thickness, high peel strength, firm feel, good resilience, and outstanding water washability, so that the mirror synthetic leather is placed in a high temperature and high humidity environment for more than 6 months without fogging, and has excellent comprehensive performance.
[0094] The difference between Example 1 and Comparative Example 2 lies in the difference in chain extenders. The use of 1,3-BG is more capable of improving the peel strength, firmness and rebound of the product than DEG, and the water washing performance is particularly outstanding.
[0095] A comparison of Example 1 and Example 3 shows that by selecting a polyether polyol with a molecular weight of 4000, a specific polypropylene oxide and ethylene oxide mixed structure, synthetic leather products can achieve better resilience, uniform solidification thickness, and improved peel strength, while also aiding in water washing. A comparison of Example 1 and Comparative Example 4 shows that by selecting a polyether polyol with a specific molecular weight of 2000, the film-forming properties and water washability of the synthetic leather base surface can be improved.
[0096] The technologies not specifically mentioned above are all referenced to the existing technologies.
[0097] With the above-described preferred embodiments of the present invention as a guide, and with reference to the above description, relevant personnel are fully capable of making various changes and modifications without departing from the technical scope of this invention. The technical scope of this invention is not limited to the contents of the specification and must be determined according to the scope of the claims.
Claims
1. A polyurethane wet process hydrolysis resistant resin for soft non-fogging mirror leather, characterized in that: The raw materials for preparation include the following components in parts by weight: 0.001-0.003 parts of inorganic acid; 175-235 parts of polyether polyol; Isocyanate 66-88 parts; 17-23 parts of small molecule alcohol; 9-12 parts of additives; 630-839 parts of solvent.
2. The polyurethane wet process hydrolysis resistant resin for soft non-fogging mirror leather according to claim 1, characterized in that: The inorganic acid is concentrated phosphoric acid.
3. The polyurethane wet process hydrolysis resistant resin for soft non-fogging mirror leather according to claim 1, characterized in that: The polyether polyols include: polyether polyols with a polytetrahydrofuran structure, polyether polyols with a mixed structure of polytetrahydrofuran and ethylene oxide, and polyether polyols with a mixed structure of polypropylene oxide and ethylene oxide; wherein the molar ratio of tetrahydrofuran units to ethylene oxide units in the polyether polyols with a mixed structure of polytetrahydrofuran and ethylene oxide is 4.5-4.8:0.1-0.2, and the molar ratio of propylene oxide units to ethylene oxide units in the polyether polyols with a mixed structure of polypropylene oxide and ethylene oxide is 2.8-3:1.8-2.
4. The polyurethane wet process hydrolysis resistant resin for soft non-fogging mirror leather according to claim 3, characterized in that: The molecular weights of the polyether polyol with a polytetrahydrofuran structure and the polyether polyol with a mixed structure of polytetrahydrofuran and ethylene oxide are both 1000-2200, and the molecular weight of the polyether polyol with a mixed structure of polypropylene oxide and ethylene oxide is 3800-4200.
5. The polyurethane wet process hydrolysis resistant resin for soft non-fogging mirror leather according to claim 1, characterized in that: The isocyanate is one or more of diphenylmethane diisocyanate, toluene diisocyanate, and dicyclohexylmethane diisocyanate.
6. The polyurethane wet process hydrolysis resistant resin for soft non-fogging mirror leather according to claim 1, characterized in that: The small molecule alcohol is one or more of 1,3-butanediol, 2-methylpropanediol and dodecanediol.
7. The polyurethane wet process hydrolysis resistant resin for soft non-fogging mirror leather according to claim 1, characterized in that: The solvent is N,N-dimethylformamide, and the auxiliary agent is one or more of a water-assisting agent, a stabilizer, a capping agent, and a hindered phenol antioxidant.
8. The polyurethane wet process hydrolysis resistant resin for soft non-fogging mirror leather according to claim 7, characterized in that: The water-assisting agent is terminal hydroxyalkyl polysiloxane, the stabilizer is benzoic acid, and the end-capping agent is methanol.
9. The method for preparing the polyurethane wet process hydrolysis resistant resin for soft non-fogging mirror leather according to any one of claims 1 to 8, characterized in that: The steps include: (1) mixing a polyether polyol having a polytetrahydrofuran structure, a polyether polyol having a mixed structure of polytetrahydrofuran and ethylene oxide, a polyether polyol having a mixed structure of polypropylene oxide and ethylene oxide, a small molecule alcohol, a hindered phenol antioxidant, an inorganic acid, and a portion of a solvent in the polyether polyol, and subjecting the mixture to a heating treatment; (2) adding a portion of isocyanate to the mixture after treatment in step (1) and treating at a constant temperature; (3) adding the remaining isocyanate to the mixture after treatment in step (2) to react, and maintaining the R value at 0.9-1.1, adding the remaining solvent until the viscosity of the reaction liquid is 20-26pas / 25 degrees, and the solid content of the reaction liquid is 30%-31%, and then adding the blocking agent, stirring, and cooling; (4) adding a stabilizer and a water-assistant to the mixture after treatment in step (3) and stirring to obtain the polyurethane wet-process hydrolysis-resistant resin.
10. A synthetic leather, characterized in that: It is prepared using the soft non-fogging polyurethane wet process hydrolysis resistant resin for mirror leather described in any one of claims 1 to 8, or is prepared using the resin prepared by the preparation method of the soft non-fogging polyurethane wet process hydrolysis resistant resin for mirror leather described in claim 9.
Citation Information
Cited By
Wet-process polyurethane resin composition, mirror-surface wet-process base, mirror-surface polyurethane synthetic leather and preparation method of mirror-surface polyurethane synthetic leather
CN121293470A