Polyisocyanate composition as well as preparation method and application thereof

By controlling the mass percentage of isocyanurate groups in the polyisocyanate composition and a specific reaction process, a polyisocyanate composition with good yellowing resistance, pendulum hardness, and drying properties was prepared. This solved the problem of poor yellowing resistance and drying properties of polyisocyanate compositions in polyurethane coatings in the prior art, and achieved an overall improvement in the coating performance.

CN118955866AActive Publication Date: 2024-11-15WANHUA CHEM GRP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411032172.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

Existing polyisocyanate compositions, when used as crosslinking agents in polyurethane coating compositions, struggle to simultaneously achieve good resistance to yellowing, pendulum hardness, and drying properties, and also suffer from uneven drying rates.

Method used

Using aliphatic diisocyanate modifiers, aliphatic-aromatic diisocyanate modifiers, and optional aromatic diisocyanate modifiers, the mass percentage of isocyanurate groups is controlled within the range of 0-10%. Through specific ratios and the use of catalysts, polyisocyanate compositions are prepared to ensure that the reaction is controlled within a suitable viscosity range.

Benefits of technology

Excellent yellowing resistance, good pendulum hardness, and suitable drying properties were achieved in the polyurethane coating composition. The yellowing resistance index of the coating was 2.2-3.2, the pendulum hardness was 0.71-0.78, and the drying time was 195-256 minutes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004970201400000033
    Figure BDA0004970201400000033
  • Figure BDA0004970201400000034
    Figure BDA0004970201400000034
  • Figure BDA0004970201400000041
    Figure BDA0004970201400000041
Patent Text Reader

Abstract

The invention relates to a polyisocyanate composition as well as a preparation method and application thereof. The polyisocyanate composition comprises an aliphatic diisocyanate modified body, an aliphatic-aromatic diisocyanate modified body and an optional aromatic diisocyanate modified body, the aliphatic diisocyanate modified body is obtained by reacting aliphatic diisocyanate; the aromatic diisocyanate modified body is obtained by reacting aromatic diisocyanate; the aliphatic-aromatic diisocyanate modified body is obtained by reacting aliphatic diisocyanate with aromatic diisocyanate; the aliphatic diisocyanate is aliphatic diisocyanate and / or alicyclic diisocyanate; when the total mass of the isocyanurate groups in the polyisocyanate composition is 100%, the mass of the isocyanurate groups contained in the aliphatic diisocyanate modified body is gt; 0 < = 10%. When the polyisocyanate composition is used in a polyurethane coating, the yellowing resistance, the swing rod hardness and the dryness of the coating can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyisocyanate compositions, and in particular relates to a polyisocyanate composition and a preparation method and application thereof. Background Art

[0002] Polyisocyanate curing agents are widely used in paint raw materials, polyurethane elastomers and polyurethane foams. Among them, aliphatic polyisocyanate curing agents containing isocyanurate groups have excellent yellowing resistance, but their products have slow drying rates, poor pendulum hardness and poor abrasion resistance; aromatic polyisocyanate curing agents containing isocyanurate groups have faster drying rates, higher hardness and excellent abrasion resistance, but due to the presence of aromatic rings, their products have poor yellowing resistance.

[0003] The polyisocyanate composition obtained by mixing aliphatic (cyclic) / aliphatic diisocyanate and aromatic diisocyanate can combine the advantages of the two to a certain extent, and obtain a polyisocyanate composition with excellent yellowing resistance, wipe resistance and drying rate. One part of the prior art is to directly mix an aliphatic diisocyanate composition containing isocyanurate groups with an aromatic polyisocyanate composition containing isocyanurate groups to obtain a polyisocyanate composition, but these polyisocyanate compositions will cause uneven drying rates due to differences in reaction rates when used as curing agents; the other part is to mix aliphatic (cyclic) / aliphatic diisocyanate monomers with aromatic diisocyanate monomers and then add a catalyst to mix and obtain a polyisocyanate composition.

[0004] CN103242254B obtains HDI-TDI polyurethane trimer by co-polymerizing TDI and HDI, which has good yellowing resistance and adhesion compared to TDI trimer, and has faster drying than HDI trimer; US4518761 provides a method for preparing a curing agent by co-polymerizing an aliphatic diisocyanate monomer and an aromatic diisocyanate monomer, but the aromatic diisocyanate monomer has high activity. If the aliphatic diisocyanate monomer and the aromatic diisocyanate monomer are directly mixed, the aromatic diisocyanate monomer will react preferentially, resulting in inability to separate. US5798431 first adds a catalyst to initiate trimerization reaction of aliphatic diisocyanate, and then drops the aromatic diisocyanate into the reaction system to solve the above problem, but the aliphatic diisocyanate is first initiated to react, resulting in a higher amount of trimer based on aliphatic diisocyanate in the system, thereby affecting the drying speed.

[0005] Therefore, it is necessary to develop a polyisocyanate composition, which can be used as a crosslinking agent for a two-component polyurethane coating composition, so that the coating can have good yellowing resistance, good pendulum hardness and drying properties. Summary of the invention

[0006] In view of the deficiencies in the prior art, the object of the present invention is to provide a polyisocyanate composition and a preparation method and application thereof. The polyisocyanate composition provided by the present invention can be used as a crosslinking agent for a two-component polyurethane coating composition, and can make the coating have good yellowing resistance, good pendulum hardness and drying properties.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a polyisocyanate composition, which comprises an aliphatic diisocyanate modifier, an aliphatic-aromatic diisocyanate modifier and optionally an aromatic diisocyanate modifier; the aliphatic diisocyanate modifier is obtained by reacting an aliphatic diisocyanate; the aromatic diisocyanate modifier is obtained by reacting an aromatic diisocyanate; the aliphatic-aromatic diisocyanate modifier is obtained by reacting an aliphatic diisocyanate with an aromatic diisocyanate; the aliphatic diisocyanate is an aliphatic diisocyanate and / or an alicyclic diisocyanate; based on the total mass of isocyanurate groups in the polyisocyanate composition being 100%, the mass of isocyanurate groups contained in the aliphatic diisocyanate modifier is >0 and ≤10%.

[0009] The polyisocyanate composition provided by the present invention is derived from aliphatic diisocyanate and aromatic diisocyanate. By controlling the mass percentage of isocyanurate groups contained in the aliphatic diisocyanate modifier within the range of >0 and ≤10% relative to the total mass of isocyanurate groups in the polyisocyanate composition, it is beneficial to improve the yellowing resistance of the polyurethane coating composition coating, and can take into account good drying performance and pendulum hardness.

[0010] The mass of isocyanurate groups contained in the aliphatic diisocyanate modifier is >0 and ≤10%, for example, it can be 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, etc.

[0011] In the present invention, the structure of the isocyanurate group is: in Represents the attachment site of the group.

[0012] In the present invention, the modified aliphatic diisocyanate comprises at least one of the following compounds:

[0013]

[0014] Wherein, R1 is independently selected from any one of C1-C20 straight chain or branched alkylene and C3-C30 cycloalkylene; n is selected from an integer ≥ 0; R1 may be the same or different.

[0015] In the present invention, the modified aromatic diisocyanate comprises at least one of the following compounds:

[0016]

[0017] Wherein, R2 is independently selected from any one of C6-C30 arylene groups; m is selected from an integer ≥ 0; and R2 may be the same or different.

[0018] In the present invention, the modified aliphatic-aromatic diisocyanate comprises at least one of the following compounds:

[0019]

[0020] Wherein, R3 is independently selected from any one of C6-C30 arylene, C1-C20 straight chain or branched alkylene, and C3-C30 cycloalkylene; p is selected from an integer ≥0; and at least one R3 is selected from any one of C6-C30 arylene, and at least one R3 is selected from any one of C1-C20 straight chain or branched alkylene or C3-C30 cycloalkylene.

[0021] In the present invention, the polyisocyanate composition may further contain any one of an iminooxadiazinedione group, a biuret group, a uretdione group, a carbamate group, an allophanate group or a uretonimine group, or a combination of at least two of them.

[0022] The structure of the iminooxadiazinedione group is: The structure of the biuret group is: The structure of the uretdione group is: The structure of the carbamate group is: The structure of the allophanate group is: The structure of the uretonimine group is: in The above structures can be detected by NMR carbon spectrum.

[0023] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.

[0024] As a preferred technical solution, the aromatic diisocyanate includes any one of toluene diisocyanate, diphenylmethane diisocyanate or meta-xylylene diisocyanate, or a combination of at least two thereof.

[0025] Preferably, the toluene diisocyanate includes any one of toluene-2,3-diisocyanate, toluene-2,4-diisocyanate, toluene-2,5-diisocyanate, toluene-2,6-diisocyanate, toluene-3,4-diisocyanate or toluene-3,5-diisocyanate, or a combination of at least two thereof.

[0026] Preferably, the aliphatic diisocyanate includes any one or a combination of at least two of tetramethylene-1,4-diisocyanate, pentamethylene-1,5-diisocyanate, hexamethylene-1,6-diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate or cyclohexane dimethylene diisocyanate.

[0027] Preferably, based on the total mass of isocyanurate groups in the polyisocyanate composition as 100%, the mass of isocyanurate groups contained in the aliphatic diisocyanate modifier is >0 and ≤8%, for example, it can be 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, etc.

[0028] Preferably, based on the total mass of isocyanurate groups in the polyisocyanate composition as 100%, the mass of isocyanurate groups contained in the aliphatic diisocyanate modifier is >0 and ≤5%, for example, it can be 0.1%, 0.3%, 0.6%, 0.9%, 1.2%, 1.6%, 1.8%, 2.2%, 2.4%, 2.6%, 2.8%, 3.2%, 3.4%, 3.6%, 3.8%, 4.2%, 4.6%, 4.8%, etc.

[0029] Controlling the mass percentage of isocyanurate groups contained in the aliphatic diisocyanate modifier within a suitable range is beneficial to further improving the yellowing resistance of the polyurethane coating composition coating, while taking into account better drying properties and pendulum hardness.

[0030] Preferably, the polyisocyanate composition further comprises an organic solvent.

[0031] Preferably, the organic solvent includes any one of ethyl acetate, n-propyl acetate, isopropyl acetate, butyl acetate or propylene glycol methyl ether acetate, or a combination of at least two thereof.

[0032] Preferably, the solid content of the polyisocyanate composition is 50-75%, for example, it can be 50%, 52%, 55%, 58%, 60%, 62%, 65%, 68%, 70%, 72%, 75%, etc.

[0033] Preferably, the viscosity of the polyisocyanate composition at 25° C. is 500-4000 cP, for example, 500 cP, 800 cP, 1000 cP, 1200 cP, 1500 cP, 1800 cP, 2000 cP, 2200 cP, 2500 cP, 2800 cP, 3000 cP, 3200 cP, 3400 cP, 3600 cP, 3800 cP, 4000 cP, etc.

[0034] Preferably, the mass percentage of isocyanate groups in the polyisocyanate composition is 8-15%, for example, it may be 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, etc.

[0035] In a second aspect, the present invention provides a method for preparing the polyisocyanate composition as described in the first aspect, the preparation method comprising the following steps:

[0036] (1) reacting aliphatic diisocyanate with part of aromatic diisocyanate to obtain reaction solution A;

[0037] (2) The reaction solution A reacts with the remaining aromatic diisocyanate to obtain the polyisocyanate composition.

[0038] Preferably, the molar ratio of the aliphatic diisocyanate to the aromatic diisocyanate is (1.5-6):1, for example, it can be 1.55:1, 1.6:1, 2:1, 2.5:1, 2.8:1, 3:1, 3.2:1, 3.4:1, 3.5:1, 3.8:1, 4:1, 4.2:1, 4.5:1, 4.8:1, 5:1, 5.2:1, 5.4:1, 5.6:1, 5.8:1, 6:1, etc.

[0039] Preferably, the molar ratio of the aliphatic diisocyanate to the aromatic diisocyanate is (2.5-4.5):1, for example, it can be 2.5:1, 2.6:1, 2.8:1, 3:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1, 4:1, 4.2:1, 4.4:1, 4.5:1, etc.

[0040] Preferably, based on the total mass of the aliphatic diisocyanate as 100%, the mass of the aromatic diisocyanate in the step (1) is 1-10%, for example, it can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, etc.

[0041] Preferably, the reaction time of step (1) is 5-30 min, for example, it can be 5 min, 6 min, 8 min, 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min, 28 min, 30 min, etc.

[0042] Preferably, the reaction temperature in step (1) is 10-150°C, for example, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc.

[0043] Preferably, the reaction in step (1) is carried out in the presence of a catalyst.

[0044] Preferably, based on the total mass of the aliphatic diisocyanate and the aromatic diisocyanate as 100%, the mass of the catalyst is 0.001-0.1% (e.g., 0.001%, 0.002%, 0.004%, 0.006%, 0.008%, 0.01%, 0.02%, 0.04%, 0.06%, 0.08%, 0.1%, etc.), more preferably 0.005-0.05wt%.

[0045] Preferably, the catalyst comprises any one of quaternary ammonium hydroxide, quaternary ammonium carboxylate, a compound containing an aminosilyl group, a tertiary amine compound or a Mannich base compound, or a combination of at least two thereof.

[0046] Preferably, the quaternary ammonium hydroxide includes any one or a combination of at least two of tetramethylammonium hydroxide, benzyltrimethylammonium hydroxide, tetraethylammonium hydroxide, dimethylethylcyclohexylammonium hydroxide and hydrates thereof.

[0047] Preferably, the quaternary ammonium carboxylate includes any one of tetramethylammonium hydroxide-2-ethylhexanoate, tetramethylammonium hydroxide-octanoate, trimethylbenzylammonium hydroxide-2-ethylhexanoate, trimethylbenzylammonium hydroxide-octanoate, tetramethylammonium hydroxide-formate, tetramethylammonium hydroxide-acetate, tetramethylammonium hydroxide-pivalate, trimethylbenzylammonium hydroxide-pivalate, tetramethylammonium hydroxide-decanoate, trimethylbenzylammonium hydroxide-decanoate, tetramethylammonium hydroxide-tetradecanoate, tetramethylammonium hydroxide-tetradecanoate, tetramethylammonium hydroxide-2-ethylhexanoate, tetramethylammonium hydroxide-octanoate, trimethylbenzylammonium hydroxide-2-ethylhexanoate, trimethylbenzylammonium hydroxide-octanoate or 2-hydroxypropyltrimethylisooctanoic acid ammonium salt or a combination of at least two thereof.

[0048] Preferably, the aminosilyl-containing compound includes any one of hexamethyldisilazane, silylamine or heptamethyldisilazane, or a combination of at least two thereof.

[0049] Preferably, the tertiary amine compound includes triethylamine and / or tripropylamine.

[0050] Preferably, the Mannich base compound comprises tris(N,N-dimethylaminomethyl)phenol.

[0051] Preferably, the reaction temperature in step (2) is 10-150°C (e.g., 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc.), more preferably 30-79°C, more preferably 45-75°C; reacting at the preferred reaction temperature can take into account good operational safety.

[0052] Preferably, when the reaction in step (2) is carried out until the viscosity of the reaction system is 40-130 cP at 25°C (for example, 40 cP, 45 cP, 50 cP, 55 cP, 60 cP, 65 cP, 70 cP, 75 cP, 80 cP, 85 cP, 90 cP, 95 cP, 100 cP, 105 cP, 110 cP, 115 cP, 120 cP, 125 cP, etc.), a terminator is added.

[0053] In the process of preparing the polyisocyanate composition, step (2) monitors the viscosity of the reaction system. When the viscosity at 25° C. is greater than 130 cP / h, the viscosity of the prepared polyisocyanate composition is often too high, which has an adverse effect on the downstream construction convenience and the leveling of the paint film. When the viscosity is less than 40 cP, it often leads to problems such as low conversion rate, high monomer consumption and increased energy consumption for subsequent monomer removal, and low functionality of the polyisocyanate composition.

[0054] Preferably, the terminator comprises a protic acid and / or an acylating agent.

[0055] Preferably, the protonic acid includes any one of phosphoric acid, benzoic acid, diisooctyl phosphate, p-toluenesulfonic acid or di-n-butyl phosphate, or a combination of at least two thereof.

[0056] Preferably, the acylating agent comprises isophthalic acid dichloride.

[0057] Those skilled in the art will appreciate that different types of catalysts used in the reaction system will result in different amounts of terminators. In the reaction system of the present invention, the amount of terminator added is based on the amount of the catalyst in the reaction system that makes it inactive.

[0058] After the terminator is added, the method further includes the steps of removing unreacted diisocyanate and diluting with an organic solvent.

[0059] In the present invention, the method for removing the unreacted diisocyanate comprises removing the unreacted diisocyanate by using a single-stage or multi-stage evaporator, so that the weight of the residual diisocyanate in the polyisocyanate composition is less than 0.5% of the weight of the polyisocyanate composition.

[0060] In a third aspect, the present invention provides a use of the polyisocyanate composition as described in the first aspect in a polyurethane material.

[0061] Preferably, the polyisocyanate composition is used as a crosslinking agent for a two-component polyurethane coating composition.

[0062] In a fourth aspect, the present invention provides a two-component polyurethane coating composition, wherein the two-component polyurethane coating composition comprises component A and component B; component A comprises the polyisocyanate composition as described in the first aspect; and component B comprises at least one hydroxyl-containing resin.

[0063] Preferably, the hydroxyl-containing resin includes any one of polyether polyol, polyester polyol, polyurethane polyol, polysiloxane polyol, polycarbonate polyol, polyether polyamine, polyaspartic acid, polybutadiene polyol, polyacrylate polyol or polyacrylic acid polyol, or a combination of at least two thereof.

[0064] The two-component polyurethane coating composition, except for the polyisocyanate composition provided by the present invention, can be selected according to the conventional two-component polyurethane coating composition, and the amount of each component can be selected without special restrictions.

[0065] Preferably, in the two-component polyurethane coating composition, the molar ratio of the isocyanate group of the polyisocyanate composition to the hydroxyl group of the hydroxyl-containing resin is 1:(0.9-1.1), for example, it can be 1:0.92, 1:0.94, 1:0.96, 1:0.98, 1:1, 1:1.02, 1:1.04, 1:1.06, 1:1.08, etc.

[0066] In some embodiments, in the two-component polyurethane coating composition, other components may be added to component A and / or component B according to application requirements, for example, leveling agents, other auxiliary agents, additives, etc. The specific selection and specific amount of other components may be determined according to actual application requirements.

[0067] Compared with the prior art, the present invention has the following beneficial effects:

[0068] The polyisocyanate composition provided by the present invention is applied to a polyurethane coating composition, so that the coating has excellent yellowing resistance and can take into account good pendulum hardness and drying properties; the yellowing resistance index of the coating is 2.2-3.2, the pendulum hardness is 0.71-0.78, and the drying time is 195-256 minutes. DETAILED DESCRIPTION

[0069] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0070] The sources of some components in the embodiments and comparative examples are as follows:

[0071] (1) HDI: Hexamethylene-1,6-diisocyanate, Wanhua Chemical Group Co., Ltd.

[0072] (2) PDI: pentamethylene-1,5-diisocyanate, Wanhua Chemical Group Co., Ltd.

[0073] (3) IPDI: isophorone diisocyanate, Wanhua Chemical Group Co., Ltd.;

[0074] (4) H6XDI: cyclohexane dimethylene diisocyanate, Wanhua Chemical Group Co., Ltd.;

[0075] (5) TDI-80: Toluene diisocyanate, containing about 80% 2,4-toluene diisocyanate and 20% 2,6-toluene diisocyanate, Wanhua Chemical Group Co., Ltd.

[0076] (6) TDI-100: Toluene diisocyanate, containing about 100% 2,4-toluene diisocyanate, Wanhua Chemical Group Co., Ltd.

[0077] (7) XDI: m-xylylenediisocyanate, Wanhua Chemical Group Co., Ltd.

[0078] (8) 2-Hydroxypropyltrimethylisooctanoate ammonium salt: Evonik Company;

[0079] (9) Benzyltrimethylammonium hydroxide: Inotech Technology Co., Ltd.;

[0080] (10) Di-n-butyl phosphate: Aladdin Reagent Company;

[0081] (11) p-Toluenesulfonic acid: Aladdin Reagent Company;

[0082] (12) Hydroxyl-containing resin: HS-129 / 70AB, Sabis HS-Co., Ltd.

[0083] Where specific experimental steps or conditions are not specified in the examples, the experiments can be carried out according to the corresponding conventional experimental steps or conditions in the technical field; reagents or instruments used without indicating the manufacturer can be obtained by purchase.

[0084] Example 1

[0085] A polyisocyanate composition, comprising an HDI modified body, an HDI-TDI modified body and a TDI modified body; based on the total mass of isocyanurate groups in the polyisocyanate composition being 100%, the mass of isocyanurate groups contained in the HDI modified body is 1.6%;

[0086] The preparation method of the polyisocyanate composition comprises the following steps:

[0087] (1) 1010 g HDI and 50 g TDI-100 were added to a reaction kettle, stirred and heated to 60° C. under a nitrogen atmosphere, and 1.02 g of a 20% n-butanol solution of 2-hydroxypropyltrimethylisooctanoic acid ammonium salt was dropwise added to the system, and the reaction was carried out for 10 min to obtain a reaction solution A;

[0088] (2) 300 g of TDI-100 was added dropwise to the reaction solution A. After the addition was completed, the reaction was carried out at 60° C., and the viscosity of the reaction solution was tracked and measured. When the viscosity reached 60 cP / 25° C., 0.20 g of di-n-butyl phosphate was added to terminate the reaction. The reaction solution was separated using a short-path evaporator (separation temperature 160° C., pressure 30 Pa) to remove unreacted diisocyanate, and the heavy components were dissolved with butyl acetate to obtain the polyisocyanate composition.

[0089] Example 2

[0090] A polyisocyanate composition, comprising a PDI modified body, a PDI-TDI modified body and a TDI modified body; based on the total mass of isocyanurate groups in the polyisocyanate composition being 100%, the mass of isocyanurate groups contained in the PDI modified body is 0.8%;

[0091] The preparation method of the polyisocyanate composition comprises the following steps:

[0092] (1) 780 g of PDI and 50 g of TDI-100 were added to a reaction kettle, stirred and heated to 55° C. under a nitrogen atmosphere, and 0.28 g of a 20% n-butanol solution of 2-hydroxypropyltrimethylisooctanoic acid ammonium salt was dropwise added to the system, and the reaction was carried out for 5 min to obtain a reaction solution A;

[0093] (2) 300 g of TDI-100 was added dropwise to the reaction solution A. After the addition was completed, the reaction was carried out at 55° C., and the viscosity of the reaction solution was tracked and measured. When the viscosity reached 42 cP / 25° C., 0.05 g of di-n-butyl phosphate was added to terminate the reaction. The reaction solution was separated using a short-path evaporator (separation temperature 150° C., pressure 24 Pa) to remove unreacted diisocyanate, and the heavy components were dissolved with butyl acetate to obtain the polyisocyanate composition.

[0094] Example 3

[0095] A polyisocyanate composition, comprising a PDI modified body, a PDI-XDI modified body and an XDI modified body; based on the total mass of isocyanurate groups in the polyisocyanate composition being 100%, the mass of isocyanurate groups contained in the PDI modified body is 2.4%;

[0096] The preparation method of the polyisocyanate composition comprises the following steps:

[0097] (1) 780 g of PDI and 64 g of XDI were added to a reaction kettle, the temperature was raised to 70° C. under a nitrogen atmosphere with stirring, 1.07 g of a 25% methanol solution of benzyltrimethylammonium hydroxide was added dropwise to the system, and the reaction was carried out for 15 min to obtain a reaction solution A;

[0098] (2) 500 g of XDI was added dropwise to the reaction solution A. After the addition was completed, the reaction was carried out at 70° C., and the viscosity of the reaction solution was tracked and measured. When the viscosity reached 89 cP / 25° C., 0.27 g of di-n-butyl phosphate was added to terminate the reaction. The reaction solution was separated using a short-path evaporator (separation temperature 165° C., pressure 14 Pa) to remove unreacted diisocyanate, and the heavy components were dissolved with butyl acetate to obtain the polyisocyanate composition.

[0099] Example 4

[0100] A polyisocyanate composition, comprising an IPDI modification, an IPDI-TDI modification and a TDI modification; based on the total mass of isocyanurate groups in the polyisocyanate composition being 100%, the mass of isocyanurate groups contained in the IPDI modification is 8.4%;

[0101] The preparation method of the polyisocyanate composition comprises the following steps:

[0102] (1) 1332 g IPDI and 10 g TDI-80 were added to a reaction kettle, stirred and heated to 80° C. under a nitrogen atmosphere, and 3.76 g of a 20% n-butanol solution of 2-hydroxypropyltrimethylisooctanoic acid ammonium salt was dropwise added to the system, and the reaction was carried out for 25 min to obtain a reaction solution A;

[0103] (2) 164 g of TDI-80 was added dropwise to the reaction solution A. After the addition was completed, the reaction was carried out at 80° C., and the viscosity of the reaction solution was tracked and measured. When the viscosity reached 108 cP / 25° C., 0.75 g of p-toluenesulfonic acid was added to terminate the reaction. The reaction solution was separated using a short-path evaporator (separation temperature 185° C., pressure 24 Pa) to remove unreacted diisocyanate, and the heavy components were dissolved with butyl acetate to obtain the polyisocyanate composition.

[0104] Example 5

[0105] A polyisocyanate composition, comprising a H6XDI modified body, a TDI modified body and a H6XDI-TDI modified body; based on the total mass of isocyanurate groups in the polyisocyanate composition being 100%, the mass of isocyanurate groups contained in the H6XDI modified body is 5.3%;

[0106] The preparation method of the polyisocyanate composition comprises the following steps:

[0107] (1) 970 g H6XDI and 20 g TDI-80 were added to a reaction kettle, stirred and heated to 75° C. under a nitrogen atmosphere, and 2.29 g of a 20% n-butanol solution of 2-hydroxypropyltrimethylisooctanoic acid ammonium salt was dropwise added to the system, and the reaction was carried out for 30 min to obtain a reaction solution A;

[0108] (2) 154 g of TDI-80 was added dropwise to the reaction solution A. After the addition was completed, the reaction was carried out at 75° C., and the viscosity of the reaction solution was tracked and measured. When the viscosity reached 128 cP / 25° C., 0.46 g of p-toluenesulfonic acid was added to terminate the reaction. The reaction solution was separated using a short-path evaporator (separation temperature 180° C., pressure 20 Pa) to remove unreacted diisocyanate, and the heavy components were dissolved with butyl acetate to obtain the polyisocyanate composition.

[0109] Example 6

[0110] A polyisocyanate composition, comprising an HDI modified body, an XDI modified body and an HDI-XDI modified body; based on the total mass of isocyanurate groups in the polyisocyanate composition being 100%, the mass of isocyanurate groups contained in the HDI modified body is 6.3%;

[0111] The preparation method of the polyisocyanate composition comprises the following steps:

[0112] (1) 1010 g HDI and 30 g XDI were added to a reaction kettle, stirred and heated to 65° C. under a nitrogen atmosphere, and 1.73 g of a 20% n-butanol solution of 2-hydroxypropyltrimethylisooctanoic acid ammonium salt was dropwise added to the system, and the reaction was carried out for 8 min to obtain a reaction solution A;

[0113] (2) 346 g of XDI was added dropwise to the reaction solution A. After the addition was completed, the reaction was carried out at 65° C., and the viscosity of the reaction solution was tracked and measured. When the viscosity reached 65 cP / 25° C., 0.35 g of di-n-butyl phosphate was added to terminate the reaction. The reaction solution was separated using a short-path evaporator (separation temperature 180° C., pressure 20 Pa) to remove unreacted diisocyanate, and the heavy components were dissolved with butyl acetate to obtain the polyisocyanate composition.

[0114] Example 7

[0115] A polyisocyanate composition, comprising an HDI modified body, an HDI-TDI modified body and a TDI modified body; based on the total mass of isocyanurate groups in the polyisocyanate composition being 100%, the mass of isocyanurate groups contained in the HDI modified body is 1.2%;

[0116] The preparation method of the polyisocyanate composition comprises the following steps:

[0117] (1) 336 g HDI and 16.5 g TDI-100 were added to a reaction kettle, stirred and heated to 60° C. under a nitrogen atmosphere, and 0.51 g of a 20% n-butanol solution of 2-hydroxypropyltrimethylisooctanoic acid ammonium salt was dropwise added to the system, and the reaction was carried out for 10 min to obtain a reaction solution A;

[0118] (2) 333.5 g of TDI-100 was added dropwise to the reaction solution A. After the addition was completed, the reaction was carried out at 60° C., and the viscosity of the reaction solution was tracked and measured. When the viscosity reached 60 cP / 25° C., 0.15 g of di-n-butyl phosphate was added to terminate the reaction. The reaction solution was separated using a short-path evaporator (separation temperature 160° C., pressure 30 Pa) to remove unreacted diisocyanate, and the heavy components were dissolved with butyl acetate to obtain the polyisocyanate composition.

[0119] Example 8

[0120] A polyisocyanate composition, comprising an HDI modified body, an HDI-TDI modified body and a TDI modified body; based on the total mass of isocyanurate groups in the polyisocyanate composition being 100%, the mass of isocyanurate groups contained in the HDI modified body is 2.2%;

[0121] The preparation method of the polyisocyanate composition comprises the following steps:

[0122] (1) 2688 g HDI and 132 g TDI-100 were added to a reaction kettle, stirred and heated to 60° C. under a nitrogen atmosphere, and 1.23 g of a 20% n-butanol solution of 2-hydroxypropyltrimethylisooctanoic acid ammonium salt was dropwise added to the system, and the reaction was carried out for 10 min to obtain a reaction solution A;

[0123] (2) 218 ​​g of TDI-100 was added dropwise to the reaction solution A. After the addition was completed, the reaction was carried out at 60° C., and the viscosity of the reaction solution was tracked and measured. When the viscosity reached 60 cP / 25° C., 0.24 g of di-n-butyl phosphate was added to terminate the reaction. The reaction solution was separated using a short-path evaporator (separation temperature 160° C., pressure 30 Pa) to remove unreacted diisocyanate, and the heavy components were dissolved with butyl acetate to obtain the polyisocyanate composition.

[0124] Comparative Example 1

[0125] A polyisocyanate composition, comprising an HDI modified body, a TDI modified body and an HDI-TDI modified body, wherein the mass of the isocyanurate groups contained in the HDI modified body is 17.4% based on the total mass of the isocyanurate groups in the polyisocyanate composition being 100%;

[0126] The preparation method of the polyisocyanate composition comprises the following steps:

[0127] (1) 1010 g of HDI was added to a reaction kettle, and the temperature was raised to 60° C. under a nitrogen atmosphere with stirring. 1.02 g of a 20% n-butanol solution of 2-hydroxypropyltrimethylisooctanoic acid ammonium salt was added dropwise to the system, and the reaction was carried out for 10 min to obtain a reaction solution A.

[0128] (2) 350 g of TDI was added dropwise to the reaction solution A. After the addition was completed, the reaction was carried out at 60° C., and the viscosity of the reaction solution was tracked and measured. When the viscosity reached 60 cP / 25° C., 0.20 g of di-n-butyl phosphate was added to terminate the reaction. The reaction solution was separated using a short-path evaporator (separation temperature 160° C., pressure 30 Pa) to remove unreacted diisocyanate, and the heavy components were dissolved with butyl acetate to obtain the polyisocyanate composition.

[0129] Comparative Example 2

[0130] A polyisocyanate composition, comprising a TDI modifier;

[0131] The preparation method of the polyisocyanate composition comprises:

[0132] 700 g of TDI was added into a reaction kettle, and the temperature was raised to 60° C. under a nitrogen atmosphere with stirring. 1.02 g of a 20% n-butanol solution of 2-hydroxypropyltrimethylisooctanoic acid ammonium salt was added dropwise into the system. After the addition was completed, the viscosity of the reaction liquid was tracked and measured. When the viscosity reached 60 cP / 25° C., 0.20 g of di-n-butyl phosphate was added to terminate the reaction. The reaction liquid was separated by a short-path evaporator (separation temperature 160° C., pressure 30 Pa), unreacted isocyanate monomers were removed, and heavy components were dissolved with butyl acetate to obtain the polyisocyanate composition.

[0133] Product Specifications

[0134] (1) NCO% (mass percentage of isocyanate groups): measured in accordance with GB / T 12009.4-2016;

[0135] (2) Viscosity: obtained using a BrookField DV-IPrime viscometer with an S21 rotor at 25°C;

[0136] (3) The percentage of the mass of isocyanurate groups contained in the aliphatic diisocyanate modifier to the total mass of isocyanurate groups in the polyisocyanate composition: measured by gel permeation chromatography using polystyrene as a standard sample and tetrahydrofuran as an eluent in accordance with GB / T27810-2011; the specific test conditions are as follows:

[0137] GPC equipment: Agilent1260

[0138] GPC columns: Pl1113-6520 and Pl113-6325 (Agilent)

[0139] Sample concentration: 3wt%

[0140] Mobile phase: tetrahydrofuran

[0141] Detection method: differential detector

[0142] Flow rate: 1mL / min

[0143] Column temperature: 35°C

[0144] The standard curve used polystyrene with a molecular weight range of 162-17900.

[0145] The basic indicators of the polyisocyanate compositions provided by Examples 1-8 and Comparative Examples 1-2 are listed in Table 1:

[0146] Table 1

[0147]

[0148] The ratios in Table 1 represent the percentage of the mass of the isocyanurate groups contained in the modified aliphatic diisocyanate to the total mass of the isocyanurate groups in the polyisocyanate composition.

[0149] Performance Testing

[0150] The polyisocyanate compositions provided in Examples 1-8 and Comparative Examples 1-2 were respectively mixed with a hydroxyl-containing resin (Sabis HS-129 / 70AB) at a NCO / OH molar ratio of 1:1, and then a mixed solvent of ethyl acetate / xylene (mass ratio of the two was 1:1) was added for dilution to prepare a paint, and the mass ratio of the total mass of the polyisocyanate composition and the hydroxyl-containing resin to the mixed solvent was 1:1. The prepared paints were named paint 1, paint 2, paint 3, paint 4, paint 5, paint 6, paint 7, paint 8, paint A, and paint B in sequence; the obtained paints were tested according to the following method, and the test results are shown in Table 2;

[0151] (1) Yellowing resistance: The above paint was coated on a tinplate coated with a white primer using a 150 μm wire rod with a coating thickness of 25-30 μm. The yellowing resistance of the paint film was tested after being left at room temperature for 7 days. A UV lamp with a wavelength of 313 nm and a light intensity of 200 mW / cm 2 , irradiate for 60s, test the initial L0, a0, b0 of the paint film and the L, a, b of the paint film after UV irradiation, and calculate the color difference value according to the following formula:

[0152] ΔE=[(L-L0) 2 +(a-a0) 2 +(b-b0) 2 ] 0.5 ,

[0153] Wherein, L represents the brightness after irradiation, and L0 represents the brightness before irradiation; a represents the red-green color after irradiation, and a0 represents the red-green color before irradiation; b represents the yellow-blue color after irradiation, and b0 represents the yellow-blue color before irradiation;

[0154] (2) Pendulum hardness: According to GB / T 1730, the substrate used is a glass plate;

[0155] (3) Drying time: Use a linear drying time recorder (manufacturer: BGD, model: BGD261) to test the drying time according to the national standard GB / T 1728;

[0156] Table 2

[0157] Yellowing resistance Pendulum hardness Drying time (3, 4 stages / min) Paint 1 2.2 0.74 232 Paint 2 2.4 0.73 214 Paint 3 2.2 0.71 242 Paint 4 2.8 0.77 202 Paint 5 2.8 0.78 223 Paint 6 2.3 0.72 256 Paint 7 3.2 0.76 195 Paint 8 2.4 0.71 265 Paint A 2.2 0.61 288 Paint B 4.0 0.79 181

[0158] It can be seen from the test results of Table 1 and Table 2 that in the paints 1-6 obtained using the polyisocyanate compositions provided in Examples 1-6, the mass percentage of isocyanurate groups contained in the aliphatic diisocyanate modifier is greater than 0 and ≤10%, and the final paints can take into account excellent yellowing resistance, pendulum hardness and drying time; the paint obtained using the polyisocyanate composition provided in Example 7 has slightly poor yellowing resistance; the paint obtained using the polyisocyanate composition provided in Example 8 has slightly poor drying performance; the paint obtained using the polyisocyanate composition provided in Comparative Example 1 has poor pendulum hardness and drying performance; the paint obtained using the polyisocyanate composition provided in Comparative Example 2 has significantly poor yellowing resistance.

[0159] The applicant declares that the present invention illustrates the detailed process equipment and process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process equipment and process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A polyisocyanate composition, It is characterized in that The polyisocyanate composition includes an aliphatic diisocyanate modifier, an aliphatic-aromatic diisocyanate modifier, and optionally an aromatic diisocyanate modifier; The modified aliphatic diisocyanate is obtained by reacting an aliphatic diisocyanate; the modified aromatic diisocyanate is obtained by reacting an aromatic diisocyanate; the modified aliphatic-aromatic diisocyanate is obtained by reacting an aliphatic diisocyanate with an aromatic diisocyanate; The aliphatic diisocyanate is an aliphatic diisocyanate and / or an alicyclic diisocyanate; Based on the total mass of isocyanurate groups in the polyisocyanate composition being 100%, the mass of isocyanurate groups contained in the modified aliphatic diisocyanate is >0 and ≤10%.

2. The polyisocyanate composition according to claim 1, It is characterized in that The aromatic diisocyanate includes any one of toluene diisocyanate, diphenylmethane diisocyanate or meta-xylylene diisocyanate or a combination of at least two thereof; The aliphatic diisocyanate includes any one of tetramethylene-1,4-diisocyanate, pentamethylene-1,5-diisocyanate, hexamethylene-1,6-diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate or cyclohexane dimethylene diisocyanate, or a combination of at least two thereof.

3. The polyisocyanate composition according to claim 1, It is characterized in that Based on the total mass of isocyanurate groups in the polyisocyanate composition being 100%, the mass of isocyanurate groups contained in the modified aliphatic diisocyanate is >0 and ≤8%.

4. The polyisocyanate composition according to claim 3, It is characterized in that Based on the total mass of isocyanurate groups in the polyisocyanate composition being 100%, the mass of isocyanurate groups contained in the modified aliphatic diisocyanate is >0 and ≤5%.

5. The polyisocyanate composition according to claim 1, It is characterized in that The polyisocyanate composition further comprises an organic solvent; The solid content of the polyisocyanate composition is 50-75%; The viscosity of the polyisocyanate composition at 25° C. is 500-4000 cP; The mass percentage of isocyanate groups in the polyisocyanate composition is 8-15%.

6. A method for preparing the polyisocyanate composition according to any one of claims 1 to 5, It is characterized in that The preparation method comprises the following steps: (1) reacting aliphatic diisocyanate with part of aromatic diisocyanate to obtain reaction solution A; (2) The reaction solution A reacts with the remaining aromatic diisocyanate to obtain the polyisocyanate composition.

7. The preparation method according to claim 6, It is characterized in that The molar ratio of the aliphatic diisocyanate to the aromatic diisocyanate is (1.5-6):1; Based on the total mass of the aliphatic diisocyanate being 100%, the mass of the aromatic diisocyanate in step (1) is 1-10%; The reaction time of step (1) is 5-30 min; The reaction temperature in step (1) is 10-150°C; The reaction in step (1) is carried out in the presence of a catalyst; Based on the total mass of the aliphatic diisocyanate and the aromatic diisocyanate being 100%, the mass of the catalyst is 0.001-0.1%.

8. The preparation method according to claim 6, It is characterized in that The reaction temperature in step (2) is 10-150°C; In step (2), when the reaction is carried out until the viscosity of the reaction system is 40-130 cP at 25° C., a terminator is added; After the terminator is added, the method further includes the steps of removing unreacted diisocyanate and diluting with an organic solvent.

9. Use of the polyisocyanate composition according to any one of claims 1 to 5 in polyurethane materials.

10. A two-component polyurethane coating composition, It is characterized in that The two-component polyurethane coating composition comprises component A and component B; The component A comprises the polyisocyanate composition as described in any one of claims 1 to 5; The component B comprises at least one hydroxyl-containing resin.

Citation Information

Patent Citations

  • Preparation method of aromatic and aliphatic mixed isocyanurate curing agent

    CN103450443A

  • Polyisocyanate composition, polyurethane resin, and two-component curable polyurethane composition

    CN107636033A

  • Polyisocyanate composition obtained by mixed polymerization of aliphatic diisocyanate and aromatic diisocyanate

    CN116041643A

  • Polyisocyanate composition obtained by mixed polymerization of aliphatic diisocyanate and aromatic diisocyanate

    CN116162223A

  • High-reactivity polyisocyanate composition and preparation method thereof

    CN116239755A