Composite filler as well as preparation method and application thereof
By grafting dendritic macromolecules on the thermally conductive filler to form a composite filler with a thixotropic structure, the problem of thermally conductive filler settlement in the glue liquid is solved, the thermal conductivity and voltage resistance of the circuit substrate are improved, and batch production is ensured. stability.
Patent Information
- Application Number
- CN202410988906.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-15
AI Technical Summary
In electronic devices, thermally conductive fillers are prone to settle in the glue liquid, resulting in unstable thermal conductivity and voltage resistance of the circuit substrate and difficult to disperse, affecting the stability of batch production.
Using composite fillers including thermally conductive fillers and dendritic macromolecules grafted on the surface of thermally conductive fillers, a thixotropic structure is formed through surface activation treatment and specific coating ratio design, which improves the anti-settlement and dispersion uniformity of composite fillers, and prepares A circuit substrate with excellent thermal conductivity and voltage resistance is produced.
It effectively improves the deposition rate of composite fillers in solvent and the dispersion effect in glue liquid, ensures the thermal conductivity, voltage resistance and batch stability of the circuit substrate, and reduces the occurrence of microcracks and pores.
Smart Images

Figure BDA0004958704800000161
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electronic industry, and in particular to a composite filler and a preparation method and application thereof. Background Art
[0002] With the development trend of high power and high density of electronic devices, the heat flow generated in electronic devices is getting larger and larger, and the thermal conductivity requirements of circuit substrates are getting higher and higher. In industry, thermal conductive fillers are usually filled in the glue to improve the thermal conductivity of the circuit substrate. However, thermal conductive fillers are prone to sedimentation in the glue, resulting in poor stability of the glue, which seriously affects the stability of the thermal conductivity of the same batch of products during the production process. At the same time, thermal conductive fillers are difficult to disperse in the glue, resulting in micro cracks and micro pores in the insulation layer of the final circuit substrate, affecting the voltage resistance of the circuit substrate. Summary of the invention
[0003] Based on this, it is necessary to provide a composite filler and its preparation method and application to address the above problems. The composite filler provided by the present invention has good anti-settling properties and effectively improves the dispersion effect in the glue solution, so that the prepared circuit substrate has excellent thermal conductivity, voltage resistance and batch stability.
[0004] A composite filler comprises a thermally conductive filler and a dendritic macromolecule grafted on the surface of the thermally conductive filler, wherein the branching generation number of the dendritic macromolecule is 2 to 7, the coverage rate of the thermally conductive filler is 3% to 15%, and the deposition rate of the composite filler in a solvent is less than 3 mm / h.
[0005] In one embodiment, the branching generation number of the dendrimer is 2 to 4 generations;
[0006] and / or, the number average molecular weight of the dendrimer is 5000 to 30000;
[0007] And / or, the terminal groups of the dendrimers include at least one of hydroxyl groups and amino groups;
[0008] And / or, the branching number of the branching unit is 3-6.
[0009] In one embodiment, the dendritic macromolecule is selected from at least one of polyester branched polymers, polyamide branched polymers, polyethylenediamine branched polymers, polyethyleneglycol branched polymers and dendritic epoxy resins.
[0010] In one embodiment, the ratio of the oil absorption value of the composite filler to the oil absorption value of the thermal conductive filler is 0.90 to 0.96;
[0011] And / or, the deposition rate of the composite filler in the solvent is ≤1.5 mm / h;
[0012] And / or, the contact angle of the composite filler is 60° to 100°.
[0013] A method for preparing the composite filler as described above comprises the following steps:
[0014] Under the protective gas, the thermal conductive filler is subjected to surface activation treatment to obtain a surface activated thermal conductive filler;
[0015] Under protective gas and heating conditions, the surface activated thermal conductive filler, dendritic macromolecules, catalyst and a first organic solvent are mixed, and the composite filler is obtained after washing and drying.
[0016] In one embodiment, the mass ratio of the thermal conductive filler to the dendritic macromolecule is 1:0.05 to 1:0.3;
[0017] And / or, the heating condition is 90°C to 110°C;
[0018] And / or, the surfactant for the surface activation treatment is selected from at least one of acrylic acid, hexadioleic acid and allyl epoxy resin;
[0019] And / or, the catalyst is selected from at least one of concentrated sulfuric acid, concentrated nitric acid and imidazole.
[0020] A glue solution comprises the composite filler as described above, a resin, a curing agent and a second organic solvent.
[0021] In one embodiment, the deposition rate of the composite filler in the glue is ≤1.1 mm / h;
[0022] And / or, the ratio of the rotational viscosity of the glue at 50 rpm to the rotational viscosity of the glue at 10 rpm is 3:5 to 4:5.
[0023] In one embodiment, based on 100 parts by weight of the resin, the amount of the composite filler is 500 to 1000 parts by weight, the amount of the curing agent is 0.005 to 0.02 parts by weight, and the amount of the second organic solvent is 200 to 600 parts by weight.
[0024] A prepreg made from the above-mentioned glue.
[0025] A circuit substrate made of the prepreg as described above.
[0026] A printed circuit board made of the circuit substrate as described above.
[0027] The above-mentioned composite filler includes a thermally conductive filler and a dendritic macromolecule with specific branching units and branching generations grafted on the surface of the thermally conductive filler. Under a specific coverage rate, the molecular chains on the surface of the composite filler are entangled with each other to form a thixotropic structure, thereby improving the anti-settling property of the composite filler, achieving a deposition rate of the composite filler in the solvent of <3mm / h, and effectively adjusting the gaps between the composite fillers, thereby improving the anti-settling property and dispersion uniformity of the composite filler in the glue solution, and the resulting circuit substrate has excellent thermal conductivity, voltage resistance and batch stability. DETAILED DESCRIPTION
[0028] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.
[0030] The composite filler provided by the present invention comprises a thermally conductive filler and a dendritic macromolecule grafted on the surface of the thermally conductive filler, wherein the branching generation number of the dendritic macromolecule is 2 to 7 generations, the coverage rate of the thermally conductive filler is 3% to 15%, and the deposition rate of the composite filler in a solvent is <3 mm / h.
[0031] The above-mentioned composite filler includes a thermally conductive filler and a dendritic macromolecule with specific branching units and branching generations grafted on the surface of the thermally conductive filler. Under a specific coverage rate, the molecular chains on the surface of the composite filler are entangled with each other to form a thixotropic structure, thereby improving the anti-settling property of the composite filler, achieving a deposition rate of the composite filler in the solvent of <3mm / h, and effectively adjusting the gaps between the composite fillers, thereby improving the anti-settling property and dispersion uniformity of the composite filler in the glue solution, and the resulting circuit substrate has excellent thermal conductivity, voltage resistance and batch stability.
[0032] It should be noted that the above-mentioned coverage rate is expressed as the mass ratio of the dendritic macromolecules grafted on the surface of the thermally conductive filler to the thermally conductive filler; the test method for the deposition rate of the above-mentioned composite filler in the solvent is to weigh 300g of the composite filler and place it in a 1L standard beaker (diameter 105mm), add 500mL of one or more solvents selected from butanone, acetone, propylene glycol methyl ether acetate, and propylene glycol monomethyl ether, disperse the obtained mixed solution at 1300rmp~1600rmp for 15min, let it stand for 1h, test the height of the supernatant, and calculate the deposition rate. The deposition rate is calculated as follows: v=h / t, wherein v is the deposition rate of the composite filler in the solvent (mm / h), h is the height of the supernatant (mm), and t is the static standing time (h).
[0033] In one embodiment, the branching generation number of the dendritic macromolecule is 2 to 4 generations, which is beneficial to increase the number of branched chains, promote the entanglement between the molecular chains on the surface of the composite filler, improve the anti-settling property of the composite filler, and promote the entanglement between the molecular chains on the surface of the composite filler and the resin molecular chains in the glue, thereby improving the anti-settling property of the composite filler in the glue, and further improving the thermal conductivity and batch stability of the prepared circuit substrate.
[0034] It can be understood that the dendritic macromolecule is a highly branched macromolecule formed by repeated polymerization and linear connection of branching units, and the molecular connection form is like a tree crown. The branching generation of the dendritic macromolecule is expressed as starting from the center of the molecular structure, and each repeated cycle reaction adds a branching layer, which is a generation, and the number of cycles is the branching generation.
[0035] In one embodiment, the number average molecular weight of the dendritic macromolecule is 5000 to 30000, which is beneficial to improve the anti-settling property of the composite filler in the solvent and the glue, and further improve the thermal conductivity and batch stability of the prepared circuit substrate.
[0036] In order to promote the entanglement between the surface of the composite filler and the molecular chains of the resin, while reducing the entanglement of the branches inside the dendritic macromolecules, ensuring appropriate gaps between the composite fillers, and improving the anti-settling properties of the composite fillers in the solvent and the glue, thereby improving the thermal conductivity and batch stability of the prepared circuit substrate, the branching number of the branching unit is preferably 3 to 6.
[0037] More preferably, the branching number of the branching unit is 3-4.
[0038] It should be noted that the branching number of the branching unit is represented by the number of molecular chains in the branching unit that contain groups that can undergo branching and chain extension reactions.
[0039] To further improve the stability and uniformity of the glue, the dendritic macromolecule preferably has at least one of a hydroxyl group and an amino group at the end of the molecular chain, which is conducive to the formation of hydrogen bonds between the composite fillers and further improves the anti-settling property and dispersion uniformity of the composite fillers in the glue.
[0040] Specifically, the dendritic macromolecule is selected from at least one of polyester branched polymers, polyamide branched polymers, polyethylenediamine branched polymers, polyethyleneglycol branched polymers, and dendritic epoxy resins.
[0041] In one embodiment, the ratio of the oil absorption value of the composite filler to the oil absorption value of the thermally conductive filler is 0.90 to 0.96, which is beneficial to ensure that the surface of the composite filler has a suitable number of branched chains, promote the entanglement between the molecular chains on the surface of the composite filler, improve the anti-settling property of the composite filler in the solvent, and promote the entanglement between the molecular chains on the surface of the composite filler and the resin molecular chains in the glue, thereby improving the anti-settling property of the composite filler in the glue, and further improving the thermal conductivity, voltage resistance and batch stability of the circuit substrate.
[0042] In order to further improve the anti-settling property and uniform dispersion of the composite filler in the glue solution, and thereby improve the excellent thermal conductivity, voltage resistance and batch stability of the prepared circuit substrate, the deposition rate of the composite filler in the solvent is preferably <2 mm / h.
[0043] More preferably, the deposition rate of the composite filler in the solvent is ≤1.5 mm / h.
[0044] In one embodiment, the contact angle of the composite filler is 60° to 100°, which is beneficial to ensure that the composite filler has suitable lipophilicity and solvent wettability, thereby improving the mutual entanglement of molecular chains on the surface of the composite filler, improving the anti-settling property of the composite filler in the solvent, and promoting the entanglement of molecular chains on the surface of the composite filler and resin molecular chains in the glue, thereby improving the anti-settling property of the composite filler in the glue, and further improving the thermal conductivity, voltage resistance and batch stability of the manufactured circuit substrate.
[0045] Preferably, the contact angle of the composite filler is 80° to 90°.
[0046] In one embodiment, the thermally conductive filler is selected from at least one of aluminum oxide, aluminum nitride, boron nitride, silicon nitride, diamond powder, magnesium oxide and zinc oxide.
[0047] In one embodiment, the coverage rate of the thermally conductive filler is preferably 5% to 7%, which is conducive to achieving a specific number of long chain branches on the surface of the composite filler, promoting the entanglement between the molecular chains on the surface of the composite filler, improving the anti-settling property of the composite filler in the solvent, and promoting the entanglement of the molecular chains on the surface of the composite filler and the resin molecular chains in the glue, thereby improving the anti-settling property of the composite filler in the glue, and further improving the thermal conductivity, voltage resistance and batch stability of the prepared circuit substrate.
[0048] The present invention also provides a method for preparing the composite filler as described above, comprising the following steps:
[0049] S1. Under a protective gas, the thermal conductive filler is subjected to a surface activation treatment to obtain a surface activated thermal conductive filler;
[0050] S2. Under protective gas and heating conditions, the surface activated thermal conductive filler, dendritic macromolecules, catalyst and first organic solvent are mixed, and the composite filler is obtained after washing and drying.
[0051] In step S1, the thermally conductive filler is subjected to surface activation treatment to increase the active functional groups and reaction sites on the surface of the thermally conductive filler, which is beneficial to the grafting of dendritic macromolecules in the subsequent steps.
[0052] It should be noted that the surface activation treatment of the thermal conductive filler is carried out by existing methods in the art, which are not limited in the present invention, such as plasma treatment, surfactant treatment, etc.
[0053] Specifically, when the surface activation treatment is performed by using a surfactant, the surfactant is selected from at least one of acrylic acid, hexadioleic acid and allyl epoxy resin.
[0054] In step S2, the surface-activated thermally conductive filler is mixed with specific dendritic macromolecules under the action of a first organic solvent and a catalyst, so that the surface of the thermally conductive filler in the composite filler is grafted with dendritic macromolecules with a specific coverage rate, thereby increasing the gaps between the composite fillers under the entanglement between the long branches of the dendritic macromolecules, making the deposition rate of the composite filler in the solvent less than 3 mm / h, improving the anti-settling property of the composite filler, and ensuring the thermal conductivity of the composite filler.
[0055] Specifically, the mass ratio of the thermally conductive filler to the dendritic macromolecule is 1:0.05 to 1:0.3, which is conducive to achieving a specific coverage rate of the composite filler, improving the anti-settling property of the composite filler, and ensuring the thermal conductivity of the composite filler.
[0056] In order to promote the grafting of dendritic macromolecules on the surface of the thermal conductive filler, the heating condition is preferably 90°C to 110°C.
[0057] In one embodiment, the catalyst is selected from at least one of concentrated sulfuric acid, concentrated nitric acid and imidazole.
[0058] In one embodiment, the first organic solvent is selected from at least one of butanone, butanone and propylene glycol monomethyl ether, which is beneficial to improving the dispersibility of the thermally conductive filler and promoting the grafting of dendritic macromolecules on the surface of the thermally conductive filler.
[0059] It can be understood that the mixing method in step S2 can be stirring or shaking.
[0060] The present invention also provides an adhesive solution, comprising the composite filler, resin, curing agent and second organic solvent as described above, so that the dendritic macromolecular chains on the surface of the composite filler will be entangled with the molecular chains on the surfaces of other composite fillers and the long chains of resin macromolecules in the adhesive solution to form a thixotropic structure to achieve the effect of slowing down sedimentation, so that the composite filler has good anti-settling and dispersion uniformity in the adhesive solution, and the adhesive solution has good uniformity and stability.
[0061] In one embodiment, based on 100 parts by weight of the resin, the amount of the composite filler is 500 to 1000 parts by weight, the amount of the curing agent is 0.005 to 0.02 parts by weight, and the amount of the second organic solvent is 200 to 800 parts by weight.
[0062] It should be noted that the resin, curing agent and second solvent of the present invention are all commonly used ingredients in the field, and the present invention has no special restrictions on this. For example, the resin is selected from at least one of epoxy resin, toughening resin, hydrocarbon resin, polyphenylene ether resin, cyanate resin, maleimide resin and BT resin; the curing agent is selected from at least one of phenolic resin, maleic anhydride, diaminodiphenyl sulfone, peroxide, azobisisobutyronitrile, imidazole, diaminodiphenylmethane, active ester and dicyandiamide; the second solvent is selected from at least one of acetone, butanone, methyl ethyl ketone, cyclohexanone, toluene or xylene, propylene glycol methyl ether, methyl ethyl ketone and propylene glycol methyl ether acetate.
[0063] In one embodiment, when the resin is selected from epoxy resin, the end groups of the dendritic macromolecules in the composite filler preferably include at least one of amino, hydroxyl, carboxyl, anhydride and epoxy groups, so that during the curing process of the resin, the dendritic macromolecules can act as a curing agent to participate in the reaction and cross-link to the main chain structure, absorb fracture energy and improve the impact resistance and heat resistance of the prepared circuit substrate.
[0064] In one embodiment, the adhesive solution further includes an auxiliary agent, and the auxiliary agent is selected from at least one of an antioxidant, a coupling agent, a dispersant, a leveling agent, a defoaming agent, and a cross-linking agent.
[0065] It should be noted that the above-mentioned auxiliary agents are common ingredients in the art, and those skilled in the art can select them according to actual needs, and the present invention has no special restrictions on this.
[0066] In one embodiment, the deposition rate of the composite filler in the glue solution is ≤1.1 mm / h.
[0067] Specifically, the test method for the deposition rate of the above-mentioned composite filler in the adhesive solution is to adjust the viscosity of the adhesive solution composed of the above-mentioned resin, curing agent and second solvent to 2900cps~3100cps, and then disperse it at a speed of 1300rmp~1600rmp in a closed environment for 30 minutes, let it stand for 1 hour, test the height of the upper clear liquid, and calculate the deposition rate. The calculation formula of the deposition rate is: v=h / t, wherein v is the deposition rate of the composite filler in the adhesive solution (mm / h), h is the height of the upper clear liquid (mm), and t is the static standing time (h).
[0068] In one embodiment, the ratio of the rotational viscosity of the glue at 50 rpm to the rotational viscosity of the glue at 10 rpm is 3:5 to 4:5, which is beneficial to improving the uniformity of the glue and the leveling during the production process, thereby reducing cracks and pores inside the manufactured circuit substrate, and is beneficial to improving the voltage resistance and thermal conductivity of the circuit substrate.
[0069] It can be understood that when the glue is coated or extruded into a film, when the components in the glue are subjected to shear force, the entanglement of the molecular chains between the composite fillers and the chain entanglement formed between the composite fillers and the resinous macromolecules are pulled apart, the connection structure is destroyed, and the viscosity decreases. When the shear force disappears, the entanglement and hydrogen bonds can be slowly formed again. The reformation process allows the glue to have a longer flow time and leveling, thereby reducing cracks and pores in the prepared circuit substrate, which is beneficial to improving the voltage resistance performance of the circuit substrate.
[0070] The present invention also provides a prepreg made by using the above-mentioned glue solution, and the prepreg has good surface uniformity.
[0071] It should be noted that the prepreg in the present invention can be prepared by an existing method, and the present invention does not limit this. Preferably, after the above-mentioned glue solution is mixed evenly, it is impregnated or coated on the reinforcing material, and dried in an oven at 120°C to 180°C for 1.5min to 6min to obtain an impregnated prepreg or a coated prepreg, and the reinforcing material is preferably at least one of glass fiber cloth, aramid cloth, PET film and carbon fiber cloth; the coated prepreg can choose whether to peel off the reinforcing material according to actual use requirements, that is, the coated prepreg can include the reinforcing material or not.
[0072] The present invention also provides a circuit substrate made of the prepreg as described above, wherein the circuit substrate has excellent thermal conductivity, voltage resistance and batch stability.
[0073] In one embodiment, the circuit substrate includes an insulating layer and a conductive layer arranged on at least one surface of the insulating layer, wherein the insulating layer is pressed from one or more superimposed impregnated semi-cured sheets as described above, and the conductive layer is selected from conductive materials such as copper foil and aluminum foil, and the present invention is not limited to this.
[0074] In another embodiment, the circuit substrate includes an insulating layer, a metal plate arranged on one surface of the insulating layer, and a conductive layer arranged on the other surface of the insulating layer, wherein the insulating layer is pressed from one or more superimposed coated semi-cured sheets as described above, the metal plate is selected from metal plates such as copper plates, aluminum plates, copper-aluminum alloy plates, and the conductive layer is selected from conductive materials such as copper foil and aluminum foil, and the present invention is not limited to this.
[0075] The present invention also provides a printed circuit board made of the circuit substrate as described above, which has excellent thermal conductivity, voltage resistance and batch stability and has high market application potential.
[0076] Specifically, the printed circuit board is made of the circuit substrate through processes such as drilling, hole filling, micro-etching, pre-preg, activation, acceleration, chemical copper and copper thickening.
[0077] Hereinafter, the composite filler and its preparation method and application will be further described through the following specific examples.
[0078] Example 1
[0079] 1000 parts by weight of aluminum nitride (pellets, S30) with an oil absorption value of 13.1% was placed in a plasma processor (argon atmosphere) and treated at 40KHz for 6 minutes, transferred to 1kg of acrylic acid, and stirred at 70°C at 300 rpm for 1 hour. The filler was washed and baked in an oven at 80°C for 10 hours to obtain a surface-activated filler.
[0080] The surface activated filler is dispersed in butanone, and the temperature is raised to 100°C by introducing a nitrogen protective atmosphere, and 0.2 parts by weight of concentrated sulfuric acid and 200 parts by weight of dendritic macromolecules (polyamide branched polymer, Chenyuan Molecular, CY-7832) are added, the branching generation is 3 generations, the number average molecular weight is 7700, the branching number of the branching unit is 3, and the terminal group is hydroxyl, and the reaction is stirred at 300rmp for 4 hours. After the filler is washed, it is placed in an oven at 80°C and baked for 10 hours to obtain a composite filler. The deposition rate of the composite filler in the solvent is 1mm / h, the contact angle is 80°, and the oil absorption value is 12.1%. Through infrared spectroscopy test, it is calculated that the coverage rate of the thermal conductive filler in the composite filler is 7%.
[0081] 50 parts by weight of NPEL-128R bisphenol A epoxy resin, 50 parts by weight of PNE-177 phenolic resin, 0.01 parts by weight of 2E4MI imidazole accelerator and 2 parts by weight of KH560 coupling agent are mixed, 400 parts by weight of acetone solvent are added, and the mixture is stirred and dissolved at a speed of 400 rpm. After complete dissolution, 700 parts by weight of composite filler are added, and the mixture is stirred at a speed of 1500 rpm for 0.5 h to obtain a glue solution, wherein the deposition rate of the composite filler in the glue solution is 0.8 mm / h, and the ratio of the rotational viscosity of the glue solution at 50 rpm to the rotational viscosity at 10 rpm is 3.3:5.
[0082] Example 2
[0083] 700 parts by weight of aluminum nitride (Wanhe, S30) and 300 parts by weight of aluminum oxide (Bai Tu, NS2M2), with an oil absorption value of 14.7%, were placed in a plasma processor (argon atmosphere), treated at 40KHz for 6 minutes, transferred to 1kg of acrylic acid, and stirred at 300rmp for 1 hour at 70°C. The filler was washed and baked in an oven at 80°C for 10 hours to obtain a surface-activated filler.
[0084] The surface activated filler is dispersed in butanone, and the temperature is raised to 100°C by introducing a nitrogen protective atmosphere, and 0.2 parts by weight of concentrated sulfuric acid and 200 parts by weight of dendritic macromolecules (polyamide branched polymer, Chenyuan Molecular, CY-6826) are added, the branching generation is 2 generations, the number average molecular weight is 5900, the branching number of the branching unit is 6, and the terminal group is hydroxyl, and the reaction is stirred at 300 rpm for 4 hours. After the filler is washed, it is placed in an oven at 80°C and baked for 10 hours to obtain a composite filler. The deposition rate of the composite filler in the solvent is 1.2 mm / h, the contact angle is 85°, the oil absorption value is 13.3%, and the coverage rate of the thermal conductive filler in the composite filler is 15%.
[0085] 50 parts by weight of NPEL-128R bisphenol A epoxy resin, 50 parts by weight of PNE-177 phenolic resin, 0.01 parts by weight of 2E4MI imidazole accelerator and 1.8 parts by weight of KH560 coupling agent are mixed, 400 parts by weight of acetone solvent are added, and the mixture is stirred and dissolved at a speed of 400 rpm. After complete dissolution, 600 parts by weight of composite filler are added, and the mixture is stirred at a speed of 1500 rpm for 0.5 h to obtain a glue solution, wherein the deposition rate of the composite filler in the glue solution is 0.9 mm / h, and the ratio of the rotational viscosity of the glue solution at 50 rpm to the rotational viscosity at 10 rpm is 3.5:5.
[0086] Example 3
[0087] Take 1000 parts by weight of boron nitride (BN203) with an oil absorption value of 18%, place it in a plasma processor (argon atmosphere), treat it at 40KHz for 6 minutes, transfer it into 1kg of acrylic acid, and stir it at 300rpm at 70℃ for 1 hour. After cleaning the filler, place it in an oven at 80℃ for 10 hours to obtain a surface-activated filler.
[0088] The surface activated filler was dispersed in butanone, and the temperature was raised to 100°C by introducing a nitrogen protective atmosphere, and 0.2 parts by weight of concentrated sulfuric acid and 200 parts by weight of dendritic macromolecules (polyamide branched polymer, Chenyuan Molecular, CY-6873) were added, with a branching generation of 7, a number average molecular weight of 27400, a branching number of branching units of 3, and an amino terminal, and the reaction was stirred at 300 rpm for 4 hours. After the filler was washed, it was placed in an oven at 80°C and baked for 10 hours to obtain a composite filler. The deposition rate of the composite filler in the solvent was 1.4 mm / h, the contact angle was 67°, the oil absorption value was 17.1%, and the coverage rate of the thermal conductive filler in the composite filler was 3%.
[0089] 50 parts by weight of NPEL-128R bisphenol A epoxy resin, 50 parts by weight of PNE-177 phenolic resin, 0.01 parts by weight of 2E4MI imidazole accelerator and 1 part by weight of KH560 coupling agent are mixed, 400 parts by weight of acetone solvent are added, and the mixture is stirred and dissolved at a speed of 400 rpm. After complete dissolution, 400 parts by weight of composite filler are added, and the mixture is stirred at a speed of 1500 rpm for 0.5 h to obtain a glue solution, wherein the deposition rate of the composite filler in the glue solution is 1.1 mm / h, and the ratio of the rotational viscosity of the glue solution at 50 rpm to the rotational viscosity at 10 rpm is 3.9:5.
[0090] Example 4
[0091] The difference between Example 4 and Example 1 is that the dendritic macromolecule adopts a polyethylene glycol branched polymer (Ruixi Bio, PFD-G5-TMP-OH), which has 5 branching generations, a number average molecular weight of 19050, a branching number of 4 branching units, and a terminal group of hydroxyl; the deposition rate of the prepared composite filler in the solvent is 1.7 mm / h, the contact angle is 82°, the oil absorption value is 12.4%, and the coverage rate of the thermal conductive filler in the composite filler is 7%; the deposition rate of the composite filler in the glue is 1 mm / h, and the ratio of the rotational viscosity of the glue at 50 rpm to the rotational viscosity at 10 rpm is 3.8:5.
[0092] Example 5
[0093] The difference between Example 5 and Example 1 is that the dendritic macromolecule adopts a polyethylene glycol branched polymer (Ruixi Bio, PGD-G4-N-NH2), which has 4 branching generations, a number average molecular weight of 15000, a branching number of 4 branching units, and an amino group; the deposition rate of the prepared composite filler in the solvent is 1.6 mm / h, the contact angle is 75°, the oil absorption value is 11.8%, and the coverage rate of the thermal conductive filler in the composite filler is 14%; the deposition rate of the composite filler in the glue is 1.1 mm / h, and the ratio of the rotational viscosity of the glue at 50 rpm to the rotational viscosity at 10 rpm is 3.8:5.
[0094] Example 6
[0095] The difference between Example 6 and Example 2 is that the addition amount of the dendritic macromolecule is 80 parts by weight, the deposition rate of the prepared composite filler in the solvent is 1.9 mm / h, the contact angle is 55°, the oil absorption value is 14%, and the coverage rate of the thermal conductive filler in the composite filler is 5%; the deposition rate of the composite filler in the glue is 1.3 mm / h, and the ratio of the rotational viscosity of the glue at 50 rpm to the rotational viscosity at 10 rpm is 4.2:5.
[0096] Example 7
[0097] The difference between Example 7 and Example 1 is that the addition amount of the dendritic macromolecule is 300 parts by weight, the deposition rate of the prepared composite filler in the solvent is 1.2 mm / h, the contact angle is 90°, the oil absorption value is 11.7%, and the coverage rate of the thermal conductive filler in the composite filler is 15%; the deposition rate of the composite filler in the glue is 1 mm / h, and the ratio of the rotational viscosity of the glue at 50 rpm to the rotational viscosity at 10 rpm is 3.2:5.
[0098] Example 8
[0099] The difference between Example 8 and Example 1 is that the dendritic macromolecule adopts a polyester branched polymer (Ruixi Bio, PFD-G4-PCL-OH), which has 4 branching generations, a number average molecular weight of 12300, a branching number of 6 branching units, and a terminal group of hydroxyl; the deposition rate of the prepared composite filler in the solvent is 1.4 mm / h, the contact angle is 75°, the oil absorption value is 12.1%, and the coverage rate of the thermal conductive filler in the composite filler is 7%; the deposition rate of the composite filler in the glue is 1.2 mm / h, and the ratio of the rotational viscosity of the glue at 50 rpm to the rotational viscosity at 10 rpm is 4:5.
[0100] Comparative Example 1
[0101] The difference between Comparative Example 1 and Example 1 is that the dendritic macromolecule adopts a polyamide branched polymer (Xinqiao Bio, PAMAM G1-OH dendrimer), the branching generation of which is 1 generation, the number average molecular weight is 5200, the branching number of the branching unit is 6, and the end group is hydroxyl; the deposition rate of the prepared composite filler in the solvent is 3.3 mm / h, the contact angle is 60°, the oil absorption value is 12.8%, and the coverage rate of the thermal conductive filler in the composite filler is 7%; the deposition rate of the composite filler in the glue is 1.8 mm / h, and the ratio of the rotational viscosity of the glue at 50 rpm to the rotational viscosity at 10 rpm is 4:5.
[0102] Comparative Example 2
[0103] The difference between Comparative Example 2 and Example 1 is that the dendritic macromolecule adopts a polyamide branched polymer (Xinqiao Bio, PAMAM G8-OH dendrimer), which has 8 branching generations, a number average molecular weight of 35,000, a branching number of 3 branching units, and a terminal group of hydroxyl; the deposition rate of the prepared composite filler in the solvent is 2.5 mm / h, the contact angle is 68°, the oil absorption value is 11.3%, and the coverage rate of the thermal conductive filler in the composite filler is 7%; the deposition rate of the composite filler in the glue is 1.2 mm / h, and the ratio of the rotational viscosity of the glue at 50 rpm to the rotational viscosity at 10 rpm is 3.9:5.
[0104] Comparative Example 3
[0105] The difference between Comparative Example 3 and Example 1 is that the addition amount of the dendritic macromolecule is 30 parts by weight; the deposition rate of the prepared composite filler in the solvent is 3.3 mm / h, the contact angle is 65°, the oil absorption value is 12.9%, and the coverage rate of the thermal conductive filler in the composite filler is 2%; the deposition rate of the composite filler in the glue is 1.4 mm / h, and the ratio of the rotational viscosity of the glue at 50 rpm to the rotational viscosity at 10 rpm is 4.1:5.
[0106] Comparative Example 4
[0107] The difference between Comparative Example 4 and Example 1 is that the addition amount of the dendritic macromolecule is 330 parts by weight; the deposition rate of the prepared composite filler in the solvent is 2.1 mm / h, the contact angle is 75°, the oil absorption value is 11.5%, and the coverage rate of the thermal conductive filler in the composite filler is 16%; the deposition rate of the composite filler in the glue is 1.3 mm / h, and the ratio of the rotational viscosity of the glue at 50 rpm to the rotational viscosity at 10 rpm is 4:5.
[0108] Comparative Example 5
[0109] The difference between Comparative Example 5 and Example 1 is that aluminum nitride (pills and, S30) is directly used in the glue solution, the deposition rate of aluminum nitride in the solvent is 5 mm / h, the deposition rate of aluminum nitride in the glue solution is 2 mm / h, and the ratio of the rotational viscosity of the glue solution at 50 rpm to the rotational viscosity at 10 rpm is 4.5:5.
[0110] Application Examples
[0111] The adhesive solutions prepared in all the examples and comparative examples were coated on the surface of the PET film, dried at 135° C. for 5 min, and the PET film was removed to obtain a prepreg.
[0112] Stack 10 prepregs, cover the upper and lower surfaces with release PET film, and place them in a high temperature press at a temperature of 220°C, a vacuum degree of 710 mmg, and a pressure of 15 kg / cm 2 The mixture was cured for 3 hours to obtain an insulating sheet.
[0113] Two prepregs were stacked and placed on the surface of a 1.0 mm copper plate. The top layer of the prepreg was covered with a 2 oz copper foil with a silane coupling agent layer. The prepreg was placed in a high temperature press at 220°C, vacuum 710 mmg, and pressure 25 kg / cm 2 The reaction mixture was cured for 3 hours to obtain a circuit substrate.
[0114] The circuit substrates prepared in all application examples and application comparison examples were subjected to performance tests, and the test indicators and methods are as follows:
[0115] (1) Thermal conductivity: Refer to ASTM D5470 to test the thermal conductivity of the insulation sheet;
[0116] (2) Voltage Withstand: Refer to IPC-TM-650 2.5.6.2 to test the electrical strength of the circuit board;
[0117] (3) Batch stability: 10 kg of adhesive solution was used to prepare prepregs by continuous coating. The 10 prepregs coated at the beginning and the 10 prepregs coated at the end were used to press insulating sheets respectively. The thermal conductivity of the two insulating sheets was tested according to ASTM D5470. The absolute value of the difference between the thermal conductivity of the two insulating sheets was calculated to characterize the batch stability.
[0118] The test results of all application examples and application comparison examples are shown in Table 1.
[0119] Table 1
[0120]
[0121] According to the above test results, under the same test conditions, the insulating sheets obtained in all application examples have a higher thermal conductivity, and the difference in thermal conductivity of the insulating sheets obtained from different batches of prepregs is small, and the electrical strength of the obtained circuit substrate is large. Therefore, the composite filler of the present invention has good anti-settling properties, effectively improves the dispersion effect of the composite filler in the glue, and thus the obtained circuit substrate has excellent thermal conductivity, voltage resistance and batch stability.
[0122] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0123] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A composite filler, characterized in that: The composite filler includes a thermally conductive filler and a dendritic macromolecule grafted on the surface of the thermally conductive filler, wherein the branching generation number of the dendritic macromolecule is 2 to 7 generations, the coverage rate of the thermally conductive filler is 3% to 15%, and the deposition rate of the composite filler in a solvent is <3 mm / h.
2. The composite filler according to claim 1, characterized in that: The branching generations of the dendrimer are 2 to 4; and / or, the number average molecular weight of the dendrimer is 5000 to 30000; And / or, the terminal groups of the dendrimers include at least one of hydroxyl groups and amino groups; And / or, the branching number of the branching unit is 3-6.
3. The composite filler according to claim 1 or 2, characterized in that: The dendritic macromolecule is selected from at least one of polyester branched polymers, polyamide branched polymers, polyethylenediamine branched polymers, polyethyleneglycol branched polymers and dendritic epoxy resins.
4. The composite filler according to claim 1, characterized in that: The ratio of the oil absorption value of the composite filler to the oil absorption value of the thermal conductive filler is 0.90 to 0.96; And / or, the deposition rate of the composite filler in the solvent is ≤1.5 mm / h; And / or, the contact angle of the composite filler is 60° to 100°.
5. A method for preparing a composite filler according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: Under the protective gas, the thermal conductive filler is subjected to surface activation treatment to obtain a surface activated thermal conductive filler; Under protective gas and heating conditions, the surface activated thermal conductive filler, dendritic macromolecules, catalyst and a first organic solvent are mixed, and the composite filler is obtained after washing and drying.
6. The method for preparing a composite filler according to claim 5, characterized in that: The mass ratio of the thermal conductive filler to the dendritic macromolecule is 1:0.05 to 1:0.3; And / or, the heating condition is 90°C to 110°C; And / or, the surfactant for the surface activation treatment is selected from at least one of acrylic acid, hexadioleic acid and allyl epoxy resin; And / or, the catalyst is selected from at least one of concentrated sulfuric acid, concentrated nitric acid and imidazole.
7. A glue solution, characterized in that: The adhesive comprises the composite filler according to any one of claims 1 to 4, a resin, a curing agent and a second organic solvent.
8. The glue solution according to claim 7, characterized in that: The deposition rate of the composite filler in the glue solution is ≤1.1 mm / h; And / or, the ratio of the rotational viscosity of the glue at 50 rpm to the rotational viscosity of the glue at 10 rpm is 3:5 to 4:
5.
9. The glue solution according to claim 7 or 8, characterized in that: Based on 100 parts by weight of the resin, the amount of the composite filler is 500 to 1000 parts by weight, the amount of the curing agent is 0.005 to 0.02 parts by weight, and the amount of the second organic solvent is 200 to 600 parts by weight.
10. A prepreg made from the adhesive solution as claimed in claims 7 to 9.
11. A circuit substrate made of the prepreg according to claim 10.
12. A printed circuit board made using the circuit substrate as claimed in claim 11.
Citation Information
Cited By
Efficient heat dissipation circuit board and manufacturing method thereof
CN120786813A