Preparation method of antibacterial moisture-absorption respirator mask material

By using sodium carboxymethylcellulose, epoxychlorohydrin and nanocomposite antibacterial materials in the ventilator mask material, the antibacterial hygroscopic hydrogel is formed, which solves the problems of condensation water and bacterial growth of the ventilator mask, and achieves efficient hygroscopicity and antibacterial properties improve the safety and comfort of the mask.

CN118956012APending Publication Date: 2024-11-15BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411253509.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing ventilator masks have shortcomings in the formation of condensate and bacterial growth, which leads to the risk of lung infection in patients. The existing solutions such as water collecting cups and heating pipelines are difficult to accurately regulate the temperature, increasing energy consumption and maintenance needs.

Method used

Sodium carboxymethylcellulose is used as the matrix material, combined with epoxychlorohydrin crosslinking agent, nanocomposite antibacterial material and lithium chloride, and covalent crosslinking to form an antibacterial hygroscopic hydrogel mask material, which has excellent hygroscopicity and inhibition Bacteriality and biocompatibility, and dopamine hydrochloride and ε-polylysine are introduced into the material to improve adhesion and bactericidal effect.

Benefits of technology

The preparation of antibacterial hygroscopic ventilator mask material is realized, which is highly hygroscopic, antibacterial and low cytotoxic, safe and non-toxic, can effectively prevent the formation of condensate and bacterial growth, and improve the comfort and safety of the mask.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956012A_ABST
    Figure CN118956012A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an antibacterial moisture-absorption respirator mask material, and the antibacterial moisture-absorption respirator mask material is a hydrogel mask material formed through covalent crosslinking by taking sodium carboxymethyl cellulose as a base material, taking epichlorohydrin as a cross-linking agent and taking a nano composite antibacterial material and lithium chloride as antibacterial agents. The sodium alginate and the carboxymethyl cellulose used in the invention belong to natural polysaccharide high polymer materials, have good biological safety and biocompatibility, and meet the requirements of safe use in the aspects of cytotoxicity, antibacterial property and biocompatibility. Meanwhile, sodium alginate and carboxymethylcellulose belong to environment-friendly materials and are biodegradable, environmental pollutants are reduced, and energy conservation and environmental protection are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of shape memory materials, and in particular to a method for preparing an antibacterial and moisture-absorbing respirator mask material. Background Art

[0002] A ventilator is a device that can replace, control or change a person's normal physiological breathing, increase lung ventilation, improve respiratory function, reduce the consumption of respiratory work, and save heart reserve capacity. The breathing mask of the ventilator is an important part of the ventilator system, mainly used to provide stable airflow and protect the patient's respiratory tract. The ventilator will pass the heated and humidified gas through the pipe mask into the patient's lungs. In this process, condensation occurs due to the temperature difference, and water droplets condense on the inner wall or inside the mask to form flowing condensed water. Condensed water droplets will cause discomfort on the patient's face; condensed water flows into the lungs, and the stimulation of foreign matter will cause the patient to choke and cough, which is easy to damage the lungs and respiratory mucosa, and even cause suffocation; condensed water can easily carry bacteria into the lungs and cause lung infection in patients.

[0003] At present, the main method used is to use a water collection cup to promote the drainage of pipeline condensation water, or to use a pipe with a heating wire to reduce the generation of condensation water. However, the condensation water in the water collection cup is an important place for bacterial reproduction, which is easy to increase the reproduction of bacteria in the ventilator tube, leading to lung infection in patients; it is difficult to accurately control the temperature by placing a heating guide wire, and regular inspection and maintenance are required. In addition, condensation water may still appear in winter or low temperature environments. The above two main measures have not solved the problem of condensation water in the ventilator mask very well. At present, domestic and foreign patents include using fans to accelerate the dissipation of fog, using wiping strips, adding heating devices, discharging and collecting fog water, and applying waterproof and absorbent materials, aiming to improve the comfort, safety and use effect of patients. By attaching super-hydrophilic moisture-absorbing and anti-fogging materials on the surface of the material, inhibiting the condensation of condensation water and absorbing it, the formation of condensation water in the respiratory tube can be fundamentally eliminated. In addition, by adding an antibacterial layer to the surface of the ventilator mask, bacterial growth can be reduced and the incidence of infection can be reduced.

[0004] In practical applications, water collection cups and heating pipelines are mainly used to manage ventilator condensate. The water collection cup is prone to accumulation of condensate due to incomplete or untimely dumping. The long-term accumulation of condensate is prone to bacterial reproduction, increasing the reproduction of bacteria in the ventilator tube, leading to lung infection in patients. Placing a heating guide wire makes it difficult to accurately control the temperature, which requires additional energy consumption and requires regular inspection and maintenance. In addition, in winter or low temperature environments, condensate may still appear even if a heating pipeline is used. And the above two methods mainly solve the problem of condensation in the ventilator pipeline, but do not solve the problem of condensation in the mask. Therefore, it is necessary to develop a method for preparing an antibacterial and hygroscopic ventilator mask material. Summary of the invention

[0005] The purpose of the present invention is to provide an antibacterial and hygroscopic material, which is mainly used for respirator masks. The respirator mask material has excellent hygroscopicity, antibacterial properties and biocompatibility, can resist water condensation, antibacterial and extremely low cytotoxicity, and has good mechanical properties, is safe and non-toxic, so as to solve the problems existing in the above-mentioned prior art.

[0006] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0007] On the one hand, the present invention comprises a hydrogel mask material formed by covalent crosslinking using sodium carboxymethyl cellulose as a matrix material, epichlorohydrin as a crosslinking agent, and a nano-composite antibacterial material and lithium chloride as an antibacterial agent, and specifically comprising the following steps:

[0008] (1) Soaking: Soaking sodium carboxymethyl cellulose in deionized water, adding sodium hydroxide to adjust the pH value to 9-10, and stirring to obtain a matrix material;

[0009] (2) Blending: The nanocomposite antibacterial material and lithium chloride are mixed in a mass ratio to form a mixed solution, and then the swollen matrix material and the mixed solution are blended in a mass ratio, wherein the matrix material and the mixed solution are blended for 10-30 minutes to obtain a hydrogel precursor solution;

[0010] (3) Gelation: adding a crosslinking agent to the hydrogel precursor solution, wherein the amount of the crosslinking agent is 2-10 vol%, stirring for 2-10 min until the solution is uniformly dispersed, and placing the solution in a water bath to induce covalent crosslinking to obtain a reaction product;

[0011] (4) Drying: After taking out the reaction product and soaking it in deionized water, it is naturally dried and then placed in a vacuum drying oven to dry to constant weight, thereby obtaining an antibacterial and moisture-absorbing respirator mask material.

[0012] Furthermore, the preparation method of the nanocomposite antibacterial material is:

[0013] The fully swollen sodium alginate was added with 1-(3-dimethylaminopropyl) 3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide and dopamine hydrochloride in a molar ratio of 1:1.5:(1.5-3.0) in a nitrogen atmosphere in the dark for full reaction, dialyzed for 3 days and then freeze-dried;

[0014] The sodium alginate-dopamine solution and the ε-polylysine solution with a pH value of 9 are mixed in a volume ratio of 1:1 to prepare the nano-composite antibacterial material.

[0015] Furthermore, the molar ratio of the carboxyl group in the sodium alginate to the dopamine hydrochloride is 1:(0.6-2).

[0016] Furthermore, in step (2), preferably, the mixing time of the nano-composite antibacterial material and lithium chloride is controlled within 30 minutes.

[0017] Furthermore, in step (2), the blending time of the base material and the mixed liquid is controlled within 30 minutes.

[0018] Furthermore, in step (3), after the hydrogel precursor solution is stirred evenly, covalent cross-linking is initiated under the conditions of a water bath temperature of 60-70° C. and a water bath time of 2-4 h.

[0019] Furthermore, in step (4), the deionized water soaking time is 48-60 hours to fully remove unreacted raw materials and reaction by-products.

[0020] Furthermore, in step (4), the drying temperature of the vacuum drying oven is 55-65°C.

[0021] On the other hand, an antibacterial and hygroscopic respirator mask material prepared by the preparation method is made of the following components in weight percentage: 5%-15% sodium carboxymethyl cellulose matrix, 70%-90% nano-composite antibacterial material, and 5%-15% lithium chloride; the nano-composite antibacterial material includes a sodium alginate-dopamine solution and an ε-polylysine solution mixed in a volume ratio of 1:1.

[0022] The beneficial effects of the present invention are:

[0023] The present invention is an antibacterial and moisture-absorbing respirator mask material. Compared with the prior art, the present invention has the following technical effects:

[0024] 1. The present invention uses dopamine hydrochloride to modify sodium alginate to improve adhesion, increase the binding force between the polymer material and the matrix material, and prevent it from falling off and being inhaled into the patient's organs to cause health crises. At the same time, sodium alginate has excellent biocompatibility and liquid absorption capacity, which makes the polymer material have hygroscopicity.

[0025] 2. The present invention introduces an antimicrobial peptide, ε-polylysine, which has a good bactericidal effect on Escherichia coli, Staphylococcus aureus and Pseudomonas aeruginosa, and is not affected by overuse and drug resistance. It makes the polymer material have excellent antibacterial properties and prevents bacterial growth.

[0026] 3. The sodium alginate and carboxymethyl cellulose used in the present invention are natural polysaccharide polymer materials, both of which have good biosafety and biocompatibility, and their performance in terms of cytotoxicity, antibacterial properties and biocompatibility all meet the requirements for safe use. At the same time, sodium alginate and carboxymethyl cellulose are both environmentally friendly materials, biodegradable, reducing environmental pollutants, and energy-saving and environmentally friendly.

[0027] 4. The loaded lithium chloride of the present invention is that the addition of lithium chloride improves the water absorption capacity of the material and the liquid hygroscopicity at a lower regeneration temperature, the raw materials are easily available, and the operation is simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 A technical roadmap of a method for preparing an antibacterial and moisture-absorbing respirator mask material of the present invention;

[0029] Figure 2 A schematic diagram of the water retention rate of a material in a method for preparing an antibacterial and hygroscopic respirator mask material of the present invention;

[0030] Figure 3 This is a schematic diagram of the water retention rate of a material in five swelling cycles in a method for preparing an antibacterial and hygroscopic respirator mask material of the present invention. DETAILED DESCRIPTION

[0031] The present invention is further described below by means of specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.

[0032] like Figure 1 As shown:

[0033] Implementation Case 1

[0034] Sodium carboxymethyl cellulose: 7.5 g (10% of total weight)

[0035] Sodium alginate: 50 g (for preparing nanocomposite antibacterial materials)

[0036] 1-(3-Dimethylaminopropyl) 3-ethylcarbodiimide hydrochloride: 75 g (mol ratio 1.5 relative to sodium alginate)

[0037] N-Hydroxysuccinimide: 25 g (same mol ratio as 1-(3-dimethylaminopropyl) 3-ethylcarbodiimide hydrochloride)

[0038] Dopamine hydrochloride: 15 g (molar ratio 1:1 relative to sodium alginate carboxyl)

[0039] ε-polylysine solution (pH = 9): volume ratio of 1:1 to sodium alginate-dopamine solution

[0040] Lithium chloride: 7.5 g (10% of total weight)

[0041] Epichlorohydrin: 1 ml (2% of the hydrogel precursor solution)

[0042] 1. Soak 7.5 g of sodium carboxymethyl cellulose in deionized water and add sodium hydroxide to adjust the pH to 9-10.

[0043] 2. To prepare a nano-composite antibacterial material, sodium alginate was reacted with 1-(3-dimethylaminopropyl) 3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide and dopamine hydrochloride, followed by dialysis and freeze-drying.

[0044] 3. Mix the obtained sodium alginate-dopamine solution with the ε-polylysine solution.

[0045] 4. Dissolve 7.5 g of lithium chloride in a small amount of deionized water and mix with the solution obtained in step 3, and blend for 30 minutes.

[0046] 5. Add 1 ml of epichlorohydrin, stir for 5 minutes, and then crosslink in a 65°C water bath for 2 hours.

[0047] 6. The reaction product was soaked in deionized water for 48 hours to remove impurities.

[0048] 7. After natural drying, dry in a vacuum drying oven at 60°C to constant weight.

[0049] Implementation Case 2

[0050] Sodium carboxymethyl cellulose: 12.5 g (15% of total weight)

[0051] Sodium alginate: 75g

[0052] 1-(3-Dimethylaminopropyl) 3-ethylcarbodiimide hydrochloride: 113 g

[0053] N-Hydroxysuccinimide: 38 g

[0054] Dopamine hydrochloride: 25 g (molar ratio 1:0.75 relative to sodium alginate carboxyl)

[0055] ε-polylysine solution (pH = 9): volume ratio of 1:1 to sodium alginate-dopamine solution

[0056] Lithium chloride: 5 g (5% of total weight)

[0057] Epichlorohydrin: 1.5 ml (3% of the hydrogel precursor solution)

[0058] The operation steps are the same as step 1 of implementation case 1, and steps 2 and 3 of implementation case 1.

[0059] Dissolve 5 g of lithium chloride and mix with the solution obtained in step 3, and blend for 30 minutes.

[0060] 1.5 ml of epichlorohydrin was added, stirred for 7 minutes, and then crosslinked in a 68°C water bath for 3.5 hours.

[0061] The reaction product was immersed in deionized water for 55 hours.

[0062] After natural drying, the samples were dried in a vacuum drying oven at 62°C to constant weight.

[0063] Implementation Case 3

[0064] Sodium carboxymethyl cellulose: 5 g (5% of total weight)

[0065] Sodium alginate: 100g

[0066] 1-(3-Dimethylaminopropyl) 3-ethylcarbodiimide hydrochloride: 150 g

[0067] N-Hydroxysuccinimide: 50 g

[0068] Dopamine hydrochloride: 33 g (molar ratio 1:2 relative to sodium alginate carboxyl)

[0069] ε-polylysine solution (pH = 9): volume ratio of 1:1 to sodium alginate-dopamine solution

[0070] Lithium chloride: 10 g (10% of total weight)

[0071] Epichlorohydrin: 2 ml (4% of the hydrogel precursor solution)

[0072] The operation steps are the same as step 1 of implementation case 1, and steps 2 and 3 of implementation case 1;

[0073] Dissolve 10 g of lithium chloride and mix with the solution obtained in step 3, and blend for 30 minutes;

[0074] Add 2 ml of epichlorohydrin, stir for 9 minutes, and then crosslink in a 70°C water bath for 4 hours;

[0075] The reaction product was immersed in deionized water for 60 hours;

[0076] After natural drying, the samples were dried in a vacuum drying oven at 65°C to constant weight.

[0077] like Figure 2 The figure shows the initial water retention value of an antibacterial hygroscopic respirator mask material after preparation. The water retention value refers to the ability of a material to retain moisture and is usually used to measure the hygroscopic properties of materials such as hydrogels.

[0078] The water absorption rate curve of Example 1 is as follows Figure 2 As shown in the figure, the water absorption rate of the material is very fast, reaching about 200 g / g within 2 hours, and the water absorption rate reaches about 650 g / g within 12 hours. Thereafter, the water absorption rate slows down and reaches an equilibrium water absorption rate of about 700 g / g within 48 hours.

[0079] Figure 3The water absorption capacity of Example 1 after five consecutive re-expansion cycles is shown. The WRV of the material in the second cycle decreased by about 5-10% compared to the first cycle, which may be due to the formation of hydrogen bonds in the material in the first cycle. Subsequently, there was no significant further decrease in the WRV of the material in the third, fourth, and fifth cycles, which was similar to the second cycle.

[0080] Even after five cycles, the water retention rate still remained at a high level, indicating that the material has good cycle stability and long-term application potential.

[0081] Hygroscopicity test: The prepared materials were immersed in deionized water to measure the water retention value (WRV).

[0082] At each time interval, the swollen material was removed from the deionized water and weighed after removing the excess liquid on the surface of the material. WRV was calculated using equation (1):

[0083] WRV=(Wt-Wd) / Wd×100 (1)

[0084] Wt – weight of material at time t;

[0085] Wd – weight of dry material.

[0086] Reswelling kinetics test: The material was dried in a vacuum oven and then immersed in deionized water. The swollen material was taken out of the deionized water at each time interval, and the excess liquid on the surface of the material was removed and weighed. Each swelling was 24 hours, and the WRV was calculated according to equation (1). The above drying-immersion operation represents one swelling cycle, and the above swelling cycle was repeated five times using the same material.

[0087] Hydrophilicity (unit: degree, °):

[0088] Example 1-3 covalently cross-linked hydrogel: the average contact angle is 15.3°, and the standard deviation is 0.6°.

[0089] Hygroscopicity (unit: g water / g material):

[0090] Example 1-3 Covalently cross-linked hydrogel: The equilibrium water absorption rate reached about 700 g / g in 48 h, with a standard deviation of 5.17%

[0091] Antibacterial performance (unit: percentage, %):

[0092] Example 1-3 Covalently cross-linked hydrogel: The inhibitory effect on microorganisms was evaluated by drawing a bacterial growth curve. The concentration of S. aureus and E. coli bacterial solution was adjusted to 1x10 6CFU / mL, and co-cultured with the hydrogel at 37°C for 12 hours. The bacterial solution was taken at 0, 2, 4, 6, 8, 10 and 12 hours after co-culture, and the OD value was measured at 600nm on an ELISA reader. The 12h inhibition rate of Staphylococcus aureus was 80.55% on average, with a standard deviation of 1.47; the 12h inhibition rate of Escherichia coli was 80.00%, with a standard deviation of 1.13.

[0093] Biocompatibility (unit: percentage, %):

[0094] Example 1-3 Covalently cross-linked hydrogel: CCK-8 method was used to detect the cytotoxicity of hydrogel extract to L929 fibroblasts. Cell viability was calculated using the following formula: Cell viability = (ODs-ODb) / (ODc-ODb)×100%. The average cell viability on the seventh day was 96.92%, with a standard deviation of 5.3%

[0095] From the data, we can see that the material has good hydrophilicity, hygroscopicity, antibacterial properties and biocompatibility. The improvement of these properties is crucial for the management of condensed water in ventilator masks, which can improve the comfort and safety of masks and reduce the risk of bacterial growth.

[0096] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing an antibacterial and hygroscopic respirator mask material, It is characterized in that The hydrogel mask material is formed by covalent cross-linking using sodium carboxymethyl cellulose as a base material, epichlorohydrin as a cross-linking agent, and nano-composite antibacterial material and lithium chloride as antibacterial agents, and specifically includes the following steps: (1) Soaking: Soaking sodium carboxymethyl cellulose in deionized water, adding sodium hydroxide to adjust the pH value to 9-10, and stirring to obtain a matrix material; (2) Blending: The nanocomposite antibacterial material and lithium chloride are mixed in a mass ratio to form a mixed solution, and then the swollen matrix material and the mixed solution are blended in a mass ratio, wherein the matrix material and the mixed solution are blended for 10-30 minutes to obtain a hydrogel precursor solution; (3) Gelation: adding a crosslinking agent to the hydrogel precursor solution, wherein the amount of the crosslinking agent is 2-10 vol%, stirring for 2-10 min until the solution is uniformly dispersed, and placing the solution in a water bath to induce covalent crosslinking to obtain a reaction product; (4) Drying: After taking out the reaction product and soaking it in deionized water, it is naturally dried and then placed in a vacuum drying oven to dry to constant weight, thereby obtaining an antibacterial and moisture-absorbing respirator mask material.

2. The method for preparing the antibacterial and hygroscopic respirator mask material according to claim 1, It is characterized in that The preparation method of the nanocomposite antibacterial material is as follows: The fully swollen sodium alginate was added with 1-(3-dimethylaminopropyl) 3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide and dopamine hydrochloride in a molar ratio of 1:1.5:(1.5-3.0) in a nitrogen atmosphere in the dark for full reaction, dialyzed for 3 days and then freeze-dried; The sodium alginate-dopamine solution and the ε-polylysine solution with a pH value of 9 are mixed in a volume ratio of 1:1 to prepare the nano-composite antibacterial material.

3. The method for preparing the antibacterial and moisture absorbing respirator mask material according to claim 2, It is characterized in that The molar ratio of the carboxyl group in the sodium alginate to the dopamine hydrochloride is 1:(0.6-2).

4. The method for preparing the antibacterial and moisture absorbing respirator mask material according to claim 1, It is characterized in that In step (2), preferably, the mixing time of the nano-composite antibacterial material and lithium chloride is controlled within 30 minutes.

5. The method for preparing the antibacterial and moisture absorbing respirator mask material according to claim 1, It is characterized in that In step (2), the blending time of the base material and the mixed liquid is controlled within 30 minutes.

6. The method for preparing the antibacterial and moisture absorbing respirator mask material according to claim 1, It is characterized in that In step (3), after the hydrogel precursor solution is stirred evenly, covalent cross-linking is initiated under the conditions of a water bath temperature of 60-70° C. and a water bath time of 2-4 h.

7. The method for preparing the antibacterial and moisture absorbing respirator mask material according to claim 1, It is characterized in that In step (4), the deionized water soaking time is 48-60 hours to fully remove unreacted raw materials and reaction by-products.

8. The method for preparing the antibacterial and moisture absorbing respirator mask material according to claim 1, It is characterized in that In step (4), the drying temperature of the vacuum drying oven is 55-65°C.

9. An antibacterial and hygroscopic respirator mask material prepared by the preparation method according to any one of claims 1 to 7, Features: The components are made according to weight percentage: 5%-15% sodium carboxymethyl cellulose matrix, 70%-90% nano-composite antibacterial material, and 5%-15% lithium chloride; the nano-composite antibacterial material comprises a sodium alginate-dopamine solution and an ε-polylysine solution mixed in a volume ratio of 1:1.