Method for processing and modifying polypropylene
By combining crystal form regulation and stretching orientation, adding β- or α-crystalline nucleating agents and performing stretching orientation processing, the problem of insufficient performance of polypropylene at room temperature and low temperature was solved, the impact strength and rigidity of polypropylene were improved, and the low temperature performance was enhanced.
Patent Information
- Application Number
- CN202410928212.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-15
AI Technical Summary
Polypropylene has insufficient performance at room temperature and low temperature, especially poor toughness and easy brittle fracture, and the existing nucleating agents have limited effect in improving this.
Modified polypropylene products are prepared by adding β- or α-crystalline nucleating agents and performing stretching and orientation processing through a polypropylene modification method that combines crystal form regulation and stretching orientation.
It significantly improves the impact strength, rigidity, and low-temperature performance of polypropylene, alleviates the problem of low-temperature embrittlement, and simplifies the processing steps.
Smart Images

Figure BDA0004938862930000041 
Figure BDA0004938862930000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-performance preparation of polypropylene, and in particular relates to a method for processing and modifying polypropylene. Background Art
[0002] As a general-purpose thermoplastic resin, polypropylene (PP) has the advantages of good mechanical properties, non-toxicity, low relative density, heat resistance, chemical resistance, and easy processing and molding, so it is widely used in pipes, construction, automobiles, home appliances, packaging and other fields. However, PP has poor toughness, is easy to break at low temperatures, has large shrinkage during processing, poor creep resistance, slow crystallization speed, and low processing efficiency, which limits the promotion and use of PP.
[0003] Polypropylene is a semi-crystalline polymer. Its mechanical properties mainly depend on the isotactic structure of the molecular chain and the crystal form after processing into products. Therefore, α-crystal or β-crystal nucleating agents can be added during processing to regulate the crystal form, thereby improving its material properties. The α-crystal form is the most stable but has lower toughness. Therefore, the addition of polypropylene α-crystal nucleating agents will improve the tensile and bending properties of polypropylene, but its impact strength will decrease slightly. The β-crystal form is a metastable state. Polypropylene of this crystal form has good impact toughness, but its rigidity is slightly lower than that of α-crystal polypropylene. Often, after adding β-crystal nucleating agents, the impact strength of polypropylene can be greatly improved, but the tensile and bending properties will decrease at this time. At present, research on the improvement of polypropylene performance mainly relies on the addition of nucleating agents for blending, but the improvement of polypropylene performance by simply adding nucleating agents is limited, and it still cannot solve the problem of low-temperature brittleness. Therefore, there is an urgent need for a method that can further improve the room temperature and low temperature performance of polypropylene to solve the above problems. Summary of the invention
[0004] The purpose of the present invention is to overcome the problem of insufficient room temperature and low temperature performance of polypropylene, and to provide a polypropylene processing modification method based on crystal form regulation and stretching orientation synergy to improve the mechanical properties of polypropylene, especially the mechanical properties at low temperatures.
[0005] To achieve the above object, the technical solution of the present invention is as follows:
[0006] A method for processing and modifying polypropylene comprises the following steps:
[0007] (1) mixing polypropylene raw materials, additives and nucleating agents, and processing them into polypropylene profiles of desired shapes;
[0008] (2) performing stretching and orientation processing on the polypropylene profile to obtain a modified polypropylene product;
[0009] Wherein, the polypropylene raw material is selected from polypropylene or a polypropylene composition, the added amount of the nucleating agent is 0-1.0% of the mass of the polypropylene raw material; the added amount of the additive is 0-1.0% of the mass of the polypropylene raw material.
[0010] It should be noted that in the technical solution of the present invention, those skilled in the art can choose whether to add additives and what kind of additives to add according to their specific needs. In the polypropylene modification method based on crystal form regulation and stretching orientation synergy protected by the present invention, the amount of additive added can be 0.
[0011] The present invention is further configured that the polypropylene is selected from one or more of isotactic homopolypropylene, random copolymer polypropylene or impact-resistant polypropylene.
[0012] The present invention is further configured that the additive includes an antioxidant, and the antioxidant is selected from one or more of phosphate antioxidant 168, hindered phenol antioxidant 1010, hindered phenol antioxidant 1098, and hindered phenol antioxidant 1076.
[0013] The present invention is further configured such that the polypropylene composition is selected from one or more of a polypropylene composition filled with inorganic particles, a polypropylene composition added with a second additive, and a polypropylene composition filled with fibers; and the second additive includes a flame retardant.
[0014] The present invention is further configured that the nucleating agent is selected from β-crystalline polypropylene nucleating agent and / or α-crystalline polypropylene nucleating agent, wherein the α-crystalline polypropylene nucleating agent is selected from one or more of inorganic nucleating agents, sorbitol nucleating agents, (substituted) aromatic carboxylic acids and metal salts thereof, (substituted) aromatic heterocyclic phosphates, and rosin nucleating agents, and the nucleating agent is mixed in any proportion; the β-crystalline polypropylene nucleating agent is selected from one or more of inorganic salts, metal oxides, condensed aromatic hydrocarbons, organic acids and salts thereof, amides, and rare earth organic compound nucleating agents, and the nucleating agent is mixed in any proportion.
[0015] The present invention is further configured such that the nucleating agent is selected from β-crystalline polypropylene nucleating agent, and the β-crystalline polypropylene nucleating agent is selected from one or more combinations of phthalates, terephthalates, carbonates, nadic acid salts, adipates, pimelic acid salts, and amide nucleating agents.
[0016] The present invention is further configured such that the amount of the nucleating agent added is 0.01 to 0.75% of the mass of the polypropylene raw material; preferably 0.05 to 0.5%.
[0017] The present invention is further configured as follows: in step (1), the polypropylene raw material, additives and nucleating agent are fed together into a twin-screw extruder for mixing, the temperature of the twin-screw extruder is 180-240°C, the feed screw speed is 10-50 rpm, and the main engine screw speed is 50-400 rpm.
[0018] The present invention is further configured such that, in step (1), the parameters of the injection molding machine are: injection temperature 180-240° C., injection pressure 90-150 bar, holding pressure 50-125 bar, and cooling time 10-60 s.
[0019] The present invention is further configured such that in step (1), after the materials are mixed, the desired polypropylene profile is obtained by extrusion, injection molding or molding.
[0020] The present invention is further configured such that, in step (2), the stretching rate of the stretching orientation process is 0.5 to 50 mm / min, and the stretching elongation is 50% to 1200%.
[0021] The invention also provides a modified polypropylene product prepared by the method.
[0022] Compared with the prior art, the present invention has the following beneficial effects: the present invention optimizes and modifies the polypropylene raw material by the synergistic effect of crystal form regulation and stretching orientation, and the obtained polypropylene product has significantly improved mechanical properties, high impact strength, good rigidity, and good low-temperature performance, and significantly improves the disadvantage of polypropylene becoming brittle at low temperatures; the polypropylene processing modification method of the present invention is simple, has fewer processing steps, and can be widely used in the production and processing of polypropylene. DETAILED DESCRIPTION
[0023] The present invention is described in detail and completely with specific embodiments below. It should be understood that the described embodiments are only some embodiments of the present invention, rather than all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of the present invention.
[0024] The raw materials used in the following examples were directly purchased, wherein the isotactic homopolypropylene was selected from the PPH045 product of Sanjiang Petrochemical, the random copolymer polypropylene was selected from the T4401 product of Dushanzi Petrochemical, and the impact-resistant polypropylene was selected from the 0640P product of Dushanzi Petrochemical.
[0025] The twin-screw extruder was HT-32 from Nanjing Rubber & Plastic Machinery Factory, and the injection molding machine was EM-120V from Zhenxiong Machinery Co., Ltd.
[0026] The present invention provides a method for processing and modifying polypropylene, comprising the following steps:
[0027] (1) mixing polypropylene raw materials, additives and nucleating agents, and processing them into polypropylene profiles of desired shapes;
[0028] (2) performing stretching and orientation processing on the polypropylene profile to obtain a modified polypropylene product;
[0029] Wherein, the polypropylene raw material is selected from polypropylene or a polypropylene composition, the added amount of the nucleating agent is 0-1.0% of the mass of the polypropylene raw material; the added amount of the additive is 0-1.0% of the mass of the polypropylene raw material.
[0030] Furthermore, the polypropylene is selected from one or more of isotactic homopolypropylene, random copolymer polypropylene or impact polypropylene; the polypropylene is preferably isotactic homopolypropylene.
[0031] Furthermore, the amount of the nucleating agent added is 0.01-0.75% of the mass of the polypropylene raw material; more preferably 0.05-0.5%, such as 0.05%, 0.1%, 0.2%, 0.3%, 0.4% and 0.5%.
[0032] Further, the nucleating agent is selected from β-crystalline polypropylene nucleating agent and / or α-crystalline polypropylene nucleating agent, wherein the α-crystalline polypropylene nucleating agent is selected from one or more of inorganic nucleating agents, sorbitol nucleating agents, (substituted) aromatic carboxylic acids and metal salts thereof, (substituted) aromatic heterocyclic phosphates, and rosin nucleating agents, and the nucleating agent is mixed in any proportion; the β-crystalline polypropylene nucleating agent is selected from one or more of inorganic salts, metal oxides, condensed aromatic hydrocarbons, organic acids and salts thereof, amides, and rare earth organic compound nucleating agents, and the nucleating agent is mixed in any proportion.
[0033] Furthermore, the nucleating agent is selected from β-crystalline polypropylene nucleating agent, and the β-crystalline polypropylene nucleating agent is selected from one or more combinations of phthalates, terephthalates, carbonates, nadic acid salts, adipates, pimelates, and amide nucleating agents.
[0034] Furthermore, in step (1), the polypropylene raw material, additives and nucleating agent are fed together into a twin-screw extruder for mixing, the temperature of the twin-screw extruder is 180-240° C., the feed screw speed is 10-50 rpm, and the main screw speed is 50-400 rpm.
[0035] Furthermore, in step (2), the stretching rate of the stretching orientation process is 0.5 to 50 mm / min, and the stretching elongation is 50% to 1200%; the stretching elongation is preferably 100% to 900%.
[0036] The technical solution of the present invention is described in detail below in conjunction with more specific embodiments.
[0037] Example 1
[0038] Weigh 1 kg of isotactic homopolymer polypropylene and 1 g of β-nucleating agent BNA-01 and put them into a high-speed mixer for uniform mixing; extrude the uniformly mixed powder through an extruder and injection mold it into a polypropylene profile through an injection molding machine, and then use a universal testing machine to stretch it at a rate of 10 mm / min to an elongation of 700%, thereby obtaining a modified polypropylene product.
[0039] In this embodiment, a twin-screw extruder is used for extrusion, and the extrusion granulation conditions of the twin-screw extruder are as follows: the temperatures of sections 1 to 8 are 190°C, 200°C, 210°C, 210°C, 210°C, 205°C, 220°C, and 210°C respectively; the head temperature is 180°C; the feed screw speed is 20 rpm; and the main screw speed is 200 rpm. The injection molding conditions of the injection molding machine are shown in Table 1:
[0040] Table 1 Nucleated polypropylene injection molding conditions
[0041]
[0042] Example 2
[0043] Compared with Example 1, the only difference is that the β nucleating agent is replaced by the α nucleating agent DMDBS to obtain a modified polypropylene product.
[0044] Example 3
[0045] Compared with Example 1, the only difference is that no nucleating agent is added to obtain a modified polypropylene product.
[0046] Comparative Example 1
[0047] Compared with Example 1, the only difference is that the polypropylene profile obtained after injection molding is not subjected to stretching processing. It is directly injection molded into standard specimens according to the national standards GB / T1043.1-2008, GB / T1040.2-2006 and GB / T9341-2008 and subjected to mechanical property tests.
[0048] Comparative Example 2
[0049] Compared with Example 2, the only difference is that the polypropylene profile obtained after injection molding is not subjected to stretching processing. It is directly injection molded into standard specimens according to the national standards GB / T1043.1-2008, GB / T1040.2-2006 and GB / T9341-2008 and subjected to mechanical property tests.
[0050] Comparative Example 3
[0051] Compared with Example 3, the only difference is that the polypropylene profile obtained after injection molding is not subjected to stretching processing. It is directly injection molded into standard specimens according to the national standards GB / T1043.1-2008, GB / T1040.2-2006 and GB / T9341-2008 and subjected to mechanical property tests.
[0052] Example 4
[0053] Compared with Example 1, the only difference is that the β-nucleating agent is replaced by TMB-5 to obtain a modified polypropylene product.
[0054] Example 5
[0055] Compared with Example 2, the only difference is that the α nucleating agent is replaced by NX8000K to obtain a modified polypropylene product.
[0056] Embodiments 6 to 10
[0057] Compared with Example 1, the only difference is that the concentration of the added β-nucleating agent is changed from 0.1wt% to 0.025wt%, 0.05wt%, 0.75wt%, 0.2wt% and 0.5wt% respectively.
[0058] Examples 11 to 13
[0059] Compared with Example 3, the only difference is that the tensile elongation when stretched at a rate of 10 mm / min using a universal testing machine is different. Examples 4 to 6 are stretched to tensile elongation of 150%, 300%, and 900%, respectively.
[0060] Embodiments 14 to 16
[0061] Compared with Experimental Example 2, the only difference is that the tensile elongation using a universal testing machine at a rate of 10 mm / min is different. Examples 14 to 16 are stretched to tensile elongation of 150%, 300%, and 900%, respectively.
[0062] Embodiments 17 to 19
[0063] Compared with Experimental Example 1, the only difference is that the tensile elongation using a universal testing machine at a rate of 10 mm / min is different. Examples 17 to 19 are stretched to tensile elongation of 150%, 300%, and 900%, respectively.
[0064] Embodiment 20
[0065] Compared with Example 1, the only difference is that the isotactic homopolypropylene is replaced by random copolymer polypropylene.
[0066] Embodiment 21
[0067] Compared with Example 1, the only difference is that the isotactic homopolypropylene is replaced by impact-resistant polypropylene.
[0068] Comparative Example 4
[0069] Compared with Example 20, the only difference is that the polypropylene profile obtained after injection molding is not subjected to stretching processing.
[0070] Comparative Example 5
[0071] Compared with Example 21, the only difference is that the polypropylene profile obtained after injection molding is not subjected to stretching processing.
[0072] Performance Testing
[0073] The modified polypropylene product specimens prepared in each embodiment are tested according to the international punching impact, tensile and bending specimens. The impact performance of the samples is tested using a simply supported beam impact tester in accordance with GB / T1043.1-2008.
[0074] The tensile / bending properties of the samples were tested using a universal testing machine, using GB / T1040.2-2006 and GB / T9341-2008 respectively. The test results of Examples 1 to 21 and Comparative Examples 1 to 5 are shown in Table 2 below.
[0075] Table 2 Mechanical properties of polypropylene products of Examples 1 to 21 and Comparative Examples 1 to 5
[0076]
[0077] By comparing the test results of Examples 1 to 3 and Comparative Examples 1 to 3, it can be seen that the mechanical properties of the polypropylene after stretching, including the impact strength, tensile strength and flexural strength at room temperature and low temperature, are significantly higher than those of the polypropylene before stretching, and the degree of degradation of the low-temperature impact performance is significantly improved; at the same time, it is found that after adding a nucleating agent, especially after adding a β-crystalline nucleating agent, the mechanical properties of the sample stretched are better than those of the blank polypropylene after only stretching, indicating that the synergy of adding a nucleating agent and the stretching process can significantly improve the rigidity and toughness of the polypropylene.
[0078] At the same time, according to Examples 6 to 19, it can be seen that the amount of nucleating agent added in the technical solution of the present invention and the tensile elongation in the stretching process are crucial to the performance of the polypropylene product. Among them, by comparing the low-temperature impact properties of the products at different tensile elongations, it was found that the degree of degradation was relatively low. At the same time, by observing the state of the samples during the experiments with different tensile elongations and comparing the samples with different tensile elongations, it can be seen that after the start of necking, until the start of tensile hardening, the performance of the polypropylene in the necking part is relatively stable, and after the start of tensile hardening, the bending modulus and tensile strength of the polypropylene are improved while the impact strength is slightly reduced. This shows that the performance after the stretch neck is relatively stable and the hardening after necking is beneficial to improving the rigidity of polypropylene but will slightly reduce the toughness.
[0079] In summary, the method for processing and modifying polypropylene provided by the present invention is based on the coordinated method of crystal form regulation and stretching process to prepare a polypropylene product with the advantages of high toughness, good rigidity and strong low-temperature performance; and the processing and modification method is simple and can be widely used in the production and processing of polypropylene.
[0080] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent transformation or modification made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for processing and modifying polypropylene, characterized in that: The steps include: (1) Mixing polypropylene raw materials, additives and nucleating agents, and processing them into polypropylene profiles of desired shapes; (2) performing stretching and orientation processing on the polypropylene profile to obtain a modified polypropylene product; Wherein, the polypropylene raw material is selected from polypropylene or a polypropylene composition, the added amount of the nucleating agent is 0-1.0% of the mass of the polypropylene raw material; the added amount of the additive is 0-1.0% of the mass of the polypropylene raw material.
2. The method for processing and modifying polypropylene according to claim 1, characterized in that: The polypropylene is selected from one or more of isotactic homopolypropylene, random copolymer polypropylene or impact polypropylene.
3. The method for processing and modifying polypropylene according to claim 1, characterized in that: The additive includes an antioxidant, and the antioxidant is selected from one or more of phosphate antioxidant 168, hindered phenol antioxidant 1010, hindered phenol antioxidant 1098, and hindered phenol antioxidant 1076; the polypropylene composition is selected from one or more of an inorganic particle-filled polypropylene composition, a polypropylene composition added with a second additive, and a fiber-filled polypropylene composition; the second additive includes a flame retardant.
4. The method for processing and modifying polypropylene according to claim 1, characterized in that: The nucleating agent is selected from β-crystalline polypropylene nucleating agent and / or α-crystalline polypropylene nucleating agent, wherein the α-crystalline polypropylene nucleating agent is selected from one or more of inorganic nucleating agents, sorbitol nucleating agents, (substituted) aromatic carboxylic acids and their metal salts, (substituted) aromatic heterocyclic phosphates, and rosin nucleating agents, and the nucleating agent is mixed in any proportion; the β-crystalline polypropylene nucleating agent is selected from one or more of inorganic salts, metal oxides, condensed ring aromatic hydrocarbons, organic acids and their salts, amides, and rare earth organic compound nucleating agents, and the nucleating agent is mixed in any proportion.
5. The method for processing and modifying polypropylene according to claim 4, characterized in that: The nucleating agent is selected from β-crystalline polypropylene nucleating agent, and the β-crystalline polypropylene nucleating agent is selected from one or more combinations of phthalates, terephthalates, carbonates, nadic acid salts, adipates, pimelic acid salts, and amide nucleating agents.
6. The method for processing and modifying polypropylene according to claim 1, characterized in that: The amount of the nucleating agent added is 0.01 to 0.75% of the mass of the polypropylene raw material; preferably 0.05 to 0.5%.
7. The method for processing and modifying polypropylene according to claim 1, characterized in that: In step (1), the polypropylene raw material, additives and nucleating agent are fed together into a twin-screw extruder for mixing. The temperature of the twin-screw extruder is 180-240° C., the feed screw speed is 10-50 rpm, and the main screw speed is 50-400 rpm.
8. The method for processing and modifying polypropylene according to claim 7, characterized in that: In step (1), the materials are mixed and then extruded, injected or molded to obtain the desired polypropylene profile.
9. The method for processing and modifying polypropylene according to claim 1, characterized in that: In step (2), the stretching rate of the stretching orientation process is 0.5 to 50 mm / min, and the stretching elongation is 50% to 1200%.
10. A modified polypropylene product obtained according to the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Beta crystal polypropylene tensile expandable material and preparation method thereof
CN102352069A
Beta-crystal-form polypropylene strip and preparation method thereof
CN105566743A
Production of polypropylene stretched material
JP1995148837A