Water-based normal-temperature curing ceramic coating and preparation method thereof
Through the combination of water-based inorganic nanoceramic emulsion and zinc phosphate emulsion, the shortcomings of ceramic coatings in soil resistance, waterproofness, weather resistance and construction performance are solved, and high-hardness, waterproof and ultra-weather-resistant ceramic coatings are achieved, suitable for cement Decoration, protection and repair of base materials.
Patent Information
- Application Number
- CN202411180472.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing ceramic coatings have poor performance in terms of stain resistance, water resistance, weather resistance and corrosion resistance, and have poor construction performance and slow drying speed, resulting in many shortcomings in their applications in the construction and transportation fields.
Using aqueous inorganic nanoceramic emulsions and zinc phosphate emulsions as the main film forming substances, a water-based normal temperature cured ceramic coating is prepared through specific raw material ratios and process flows, including premixes of aqueous inorganic nanoceramic emulsions and zinc phosphate emulsions. , combine specific surfactants, fillers, pigments and other additives to improve the performance of the paint.
It achieves high hardness, scratch resistance, wear resistance, water resistance and super weather resistance of the paint, extends its service life, and improves its adhesion to cement-based materials, has excellent anti-carbonization and corrosion resistance, and is convenient to construct.
Smart Images

Figure BDA0005011993600000021 
Figure BDA0005011993600000022 
Figure BDA0005011993600000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, in particular to a water-based room-temperature curing ceramic coating and a preparation method thereof. Background Art
[0002] As a new type of ceramic coating suitable for cement-based surfaces, water-based ceramic coating has a wide range of applications and a strong market demand. In the field of construction, as people's requirements for the aesthetics and durability of buildings continue to increase. Ceramic coatings have gradually become the first choice for exterior wall coatings due to their excellent decorative effects and weather resistance. According to statistics, in recent years, the demand for ceramic coatings in the construction field has increased at an average annual rate of 20%, showing a huge market space.
[0003] In the field of transportation, ceramic coatings also show great application value. For example, in the anti-corrosion coating of infrastructure such as bridges and tunnels, ceramic coatings have won the favor of the market with its excellent anti-corrosion performance and construction convenience.
[0004] Room temperature curing ceramic coatings also excel in environmental performance. No high temperature treatment is required during the preparation process, achieving low volatile organic compound (VOC) emissions. At the same time, the coating is non-toxic and harmless during use, meeting environmental protection requirements. Therefore, more and more construction projects are beginning to use room temperature curing ceramic coatings to achieve green and sustainable development of buildings.
[0005] The application of ceramic coatings in cement-based materials has a significant effect, which not only improves the performance of the materials but also reduces the construction cost. As a building decoration and protection material, after practical application, its weather resistance, corrosion resistance and anti-pollution performance are excellent, effectively extending the service life of the building.
[0006] The emergence of ceramic coatings has overturned the design concept of traditional organic coatings and made it possible to realize many coating functions. However, ceramic coatings based on existing technologies also have many problems, such as:
[0007] (1) Poor stain resistance and water resistance;
[0008] (2) Poor weather resistance and corrosion resistance;
[0009] (3) The high hardness after film formation leads to average tensile strength;
[0010] (4) Poor construction performance and slow drying speed. Summary of the invention
[0011] The technical problem to be solved by the present invention is: in order to overcome the deficiencies in the prior art, a water-based room temperature curing ceramic coating and a preparation method thereof are provided.
[0012] The technical solution adopted by the present invention is: a water-based room temperature curing ceramic coating, comprising the following raw materials in percentage by mass:
[0013] Aqueous inorganic nano-ceramic emulsion premix 30-80%
[0014] Zinc phosphate emulsion premix 20-70%.
[0015] Furthermore, the aqueous inorganic nano-ceramic emulsion premix comprises the following raw materials in percentage by mass:
[0016]
[0017] Furthermore, the zinc phosphate emulsion premix comprises the following raw materials in percentage by weight:
[0018]
[0019]
[0020] Furthermore, the aqueous inorganic nano-ceramic emulsion comprises the following raw materials in percentage by mass:
[0021] Silica sol 33~55%
[0022] Organic silane 12~42%
[0023] Aqueous silicone dispersion 25-33%.
[0024] Furthermore, the silica sol is an acidic silica sol, an alkaline silica sol or a mixture of the two;
[0025] The organosilane is selected from the group consisting of methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, 3-glycidyloxypropyltrimethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, glycidoxypropylmethyldimethoxysilane, glycidoxypropylmethyldiethoxysilane, diphenyldimethoxysilane, and a mixture of two or more thereof;
[0026] The aqueous organosilicon dispersion adopts aminosilane hydrolyzate.
[0027] Further, the organosilane and aqueous organosilicon dispersion are pretreated with a surfactant;
[0028] Furthermore, the surfactant is one or a mixture of two or more of carboxylate type, sulfonate type, citrate type, sulfate (ester) type and phosphate (ester) type.
[0029] Furthermore, the filler is one or a mixture of two or more of mica powder, nano-fumed silica, kaolin, whisker silicon, micron- and nano-sized spherical alumina, calcium sulfate whisker, magnesium sulfate whisker, aluminum borate whisker and zirconium sulfate whisker;
[0030] The pigment is one or a mixture of two or more of titanium dioxide, copper chrome black, cobalt black, manganese iron black, pearlescent pigment, fluorescent pigment and metallic pigment;
[0031] The wetting and dispersing agent is BASF dispersant Dispex Ultra PX 4575.
[0032] Furthermore, the zinc phosphate emulsion is prepared by the reaction, aging, washing, filtering and emulsification of phosphate and zinc salt, and its unique chemical composition and structure significantly improve the weather resistance, corrosion resistance and adhesion of the prepared ceramic coating. In practical applications, the zinc phosphate emulsion can significantly improve the durability of cement floor coatings, making it less prone to fading and peeling, and extending its service life.
[0033] The defoamer is silicone defoamer S771;
[0034] The leveling agent is methyl silicone oil, hydroxy silicone oil or a mixture of the two;
[0035] The thickener is a special thickener for emulsified silicone oil, specifically, a special thickener for emulsified silicone oil QHY-Y905 produced by Guangzhou Zhuohou Environmental Protection Technology Co., Ltd.
[0036] The preparation method of water-based room temperature curing ceramic coating comprises the following steps:
[0037] (1) Preparation of aqueous inorganic nano-ceramic emulsion:
[0038] The first step: adding a surfactant to the organosilane and stirring evenly to obtain a pretreated organosilane; then dropping the pretreated organosilane into the silica sol, the titration time is 30 minutes, and after the titration is completed, the temperature is raised to maintain the reaction temperature at 35-70°C, and the reaction is carried out at a constant temperature for 0.5-5 hours, and then a certain amount of water is added, the heating is stopped, and the temperature is lowered to obtain a water-based silane-modified nano-silicon emulsion;
[0039] Step 2: Mix the surfactant and water to obtain a surfactant aqueous solution; then drop the aminosilane hydrolyzate into the pre-mixed surfactant aqueous solution for 30 minutes, and then continue to stir and react for 0.5 to 2 hours, then add a certain amount of water, and cool to room temperature to obtain a pre-treated aqueous silicone dispersion;
[0040] Step 3: Mix the water-based silane-modified nano-silicon emulsion obtained in the first step with the water-based organosilicon dispersion obtained in the second step in a certain proportion, and after mixing evenly, obtain a water-based inorganic nano-ceramic emulsion;
[0041] (2) Preparation of aqueous ceramic emulsion premix:
[0042] The aqueous inorganic nano-ceramic emulsion obtained in (1), as well as the filler, pigment, wetting dispersant and water are placed in a grinder and ground for 0.5 to 1.5 hours, and then transferred to a stirring tank and stirred evenly. The stirring conditions are intermittent stirring, the stirring speed is 800 to 1200 rpm, and each stirring is 10 to 20 minutes, and then the mixture is allowed to stand for 6 to 10 minutes, and the cycle is repeated 3 to 5 times. The mixture is then transferred to a high-speed disperser for dispersion, and the dispersion time is 1 to 2 hours to obtain an aqueous ceramic emulsion premix;
[0043] (3) Preparation of zinc phosphate emulsion premix:
[0044] Mix zinc phosphate emulsion, defoamer, leveling agent, thickener and water and stir evenly for 30 to 90 minutes at a stirring speed of 600 to 1000 rpm to obtain a zinc phosphate emulsion premix:
[0045] (4) Preparation of water-based room temperature curing ceramic coating:
[0046] The water-based ceramic emulsion premix obtained in (2) is added to the zinc phosphate emulsion premix obtained in (3) and mixed and ground for 0.5 to 1.5 hours, and the cooling water is adjusted so that the temperature of the ground material does not exceed 60° C. After the grinding is completed, it is filtered to obtain a water-based room temperature curing ceramic coating.
[0047] Compared with the prior art, the present invention has the following advantages:
[0048] The water-based inorganic nano-ceramic emulsion and zinc phosphate emulsion used in the present invention both have room temperature curing properties. The water-based ceramic coating prepared with the two emulsions as main film-forming substances has a room temperature curing effect during construction, and the construction is convenient;
[0049] Water-based room temperature curing ceramic coating has the characteristics of high hardness, scratch resistance, wear resistance, waterproofness, and super weather resistance. It is not easy to fade and peel off, which prolongs its service life.
[0050] Water-based room temperature curing ceramic coating can be used on the surface of any cement-based material. It has excellent adhesion, acid and alkali corrosion resistance, and has excellent anti-carbonization and anti-corrosion effects. DETAILED DESCRIPTION
[0051] The embodiments of the present invention are described in detail below. The embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following embodiments.
[0052] Example 1
[0053] The preparation method of water-based room temperature curing ceramic coating comprises the following steps:
[0054] (1) Preparation of aqueous inorganic nano-ceramic emulsion:
[0055] The first step: add 0.5 parts by mass of surfactant to 12 parts by mass of vinyltrimethoxysilane and stir evenly to obtain pretreated organic silane; then add the pretreated organic silane dropwise to 55 parts by mass of silica sol, the titration time is 30 minutes, after the titration is completed, start heating to maintain the reaction temperature at 35-70°C, react at a constant temperature for 0.5-5 hours, then add a certain amount of water, stop heating, cool down, and obtain a water-based silane-modified nano-silicon emulsion.
[0056] Step 2: Mix 0.2 parts by mass of surfactant with 80 parts by mass of water, mix them evenly to obtain a surfactant aqueous solution; then add 33 parts by mass of aminosilane hydrolyzate dropwise into the pre-stirred surfactant aqueous solution, the titration time is 30 minutes, and then continue to stir the reaction for 0.5 to 2 hours, then add a certain amount of water, and cool to room temperature to obtain a pretreated aqueous silicone dispersion.
[0057] Step 3: Mix all the aqueous silane-modified nano-silicon emulsion obtained in the first step with all the aqueous silicone dispersion obtained in the second step, and after mixing evenly, obtain an aqueous inorganic nano-ceramic emulsion.
[0058] (2) Preparation of aqueous ceramic emulsion premix:
[0059] 35 parts by mass of the aqueous inorganic nano-ceramic emulsion obtained in (1), 5 parts by mass of a filler, 1 part by mass of a pigment, 0.1 parts by mass of a wetting and dispersing agent, and 58.9 parts by mass of water are placed in a grinder and ground for 0.5 to 1.5 hours, and then transferred to a stirring tank and stirred evenly. The stirring conditions are intermittent stirring, the stirring speed is 800 to 1200 rpm, and the stirring is performed for 10 to 20 minutes, and then the mixture is allowed to stand for 6 to 10 minutes, and the cycle is repeated 3 to 5 times. The mixture is then transferred to a high-speed disperser for dispersion, and the dispersion time is 1 to 2 hours to obtain an aqueous ceramic emulsion premix.
[0060] (3) Preparation of zinc phosphate emulsion premix:
[0061] 60 parts by mass of zinc phosphate emulsion, 0.1 parts by mass of defoamer, 0.1 parts by mass of leveling agent, 1 part by mass of thickener and 38.8 parts by mass of water are mixed and stirred uniformly for 30 to 90 minutes at a stirring speed of 600 to 1000 rpm to obtain a zinc phosphate emulsion premix.
[0062] (4) Preparation of water-based room temperature curing ceramic coating:
[0063] 30 parts by mass of the aqueous ceramic emulsion premix obtained in (2) is added to 70 parts by mass of the zinc phosphate emulsion premix obtained in (3), and the mixture is mixed and ground for 0.5 to 1.5 hours, and the cooling water is adjusted so that the temperature of the ground material does not exceed 60° C. After the grinding is completed, the mixture is filtered to obtain a water-based room temperature curing ceramic coating.
[0064] Example 2
[0065] The preparation method of water-based room temperature curing ceramic coating comprises the following steps:
[0066] (1) Preparation of aqueous inorganic nano-ceramic emulsion:
[0067] The first step: add 0.5 parts by mass of a surfactant to 17 parts by mass of phenyltrimethoxysilane and stir evenly to obtain a pretreated organic silane; then drop the pretreated organic silane into 50 parts by mass of silica sol, the titration time is 30 minutes, and after the titration is completed, the temperature is raised and maintained at 35-70°C for a constant temperature reaction for 0.5-5 hours, and then a certain amount of water is added, the heating is stopped, and the temperature is cooled to obtain a water-based silane-modified nano-silicon emulsion.
[0068] Step 2: Mix 0.2 parts by mass of surfactant with 80 parts by mass of water, mix them evenly to obtain a surfactant aqueous solution; then add 33 parts by mass of aminosilane hydrolyzate dropwise into the pre-stirred surfactant aqueous solution, the titration time is 30 minutes, and then continue to stir the reaction for 0.5 to 2 hours, then add a certain amount of water, and cool to room temperature to obtain a pretreated aqueous silicone dispersion.
[0069] Step 3: Mix all the aqueous silane-modified nano-silicon emulsion obtained in the first step with all the aqueous silicone dispersion obtained in the second step, and after mixing evenly, obtain an aqueous inorganic nano-ceramic emulsion.
[0070] (2) Preparation of aqueous ceramic emulsion premix:
[0071] 40 parts by mass of the aqueous inorganic nano-ceramic emulsion obtained in (1), 10 parts by mass of a filler, 3 parts by mass of a pigment, 0.3 parts by mass of a wetting and dispersing agent, and 46.7 parts by mass of water are placed in a grinder and ground for 0.5 to 1.5 hours, and then transferred to a stirring tank and stirred evenly. The stirring conditions are intermittent stirring, the stirring speed is 800 to 1200 rpm, and the stirring is performed for 10 to 20 minutes, and then the mixture is allowed to stand for 6 to 10 minutes, and the mixture is cycled for 3 to 5 times. The mixture is then transferred to a high-speed disperser for dispersion, and the dispersion time is 1 to 2 hours to obtain an aqueous ceramic emulsion premix.
[0072] (3) Preparation of zinc phosphate emulsion premix:
[0073] 65 parts by mass of zinc phosphate emulsion, 0.15 parts by mass of defoamer, 0.1 parts by mass of leveling agent, 1.5 parts by mass of thickener and 33.2 parts by mass of water are mixed and stirred uniformly for 30 to 90 minutes at a stirring speed of 600 to 1000 rpm to obtain a zinc phosphate emulsion premix.
[0074] (4) Preparation of water-based room temperature curing ceramic coating:
[0075] 40 parts by mass of the aqueous ceramic emulsion premix obtained in (2) is added to 60 parts by mass of the zinc phosphate emulsion premix obtained in (3), and the mixture is mixed and ground for 0.5 to 1.5 hours, and the cooling water is adjusted so that the temperature of the ground material does not exceed 60° C. After the grinding is completed, the mixture is filtered to obtain a water-based room temperature curing ceramic coating.
[0076] Example 3
[0077] The preparation method of water-based room temperature curing ceramic coating comprises the following steps:
[0078] (1) Preparation of aqueous inorganic nano-ceramic emulsion:
[0079] The first step: adding 0.5 parts by mass of a surfactant to 22 parts by mass of phenyltriethoxysilane and stirring evenly to obtain a pretreated organosilane; then dropping the pretreated organosilane into 45 parts by mass of silica sol, the titration time is 30 minutes, and then after the titration is completed, the temperature is raised to maintain the reaction temperature at 35-70°C, the constant temperature reaction is performed for 0.5-5 hours, and then a certain amount of water is added, the heating is stopped, and the temperature is lowered to obtain a water-based silane-modified nano-silicon emulsion;
[0080] Step 2: 0.2 parts by mass of surfactant and 80 parts by mass of water are mixed and mixed evenly to obtain a surfactant aqueous solution; then 33 parts by mass of aminosilane hydrolyzate is added dropwise to the pre-stirred surfactant aqueous solution for 30 minutes, and then the stirring reaction is continued for 0.5 to 2 hours, and then a certain amount of water is added, and the temperature is lowered to room temperature to obtain a pre-treated aqueous silicone dispersion;
[0081] Step 3: Mix all the aqueous silane-modified nano-silicon emulsion obtained in the first step with all the aqueous silicone dispersion obtained in the second step, and after mixing evenly, obtain an aqueous inorganic nano-ceramic emulsion.
[0082] (2) Preparation of aqueous ceramic emulsion premix:
[0083] 45 parts by mass of the aqueous inorganic nano-ceramic emulsion obtained in (1), 15 parts by mass of a filler, 5 parts by mass of a pigment, 0.3 parts by mass of a wetting and dispersing agent, and 34.7 parts by mass of water are placed in a grinder and ground for 0.5 to 1.5 hours, and then transferred to a stirring tank and stirred evenly. The stirring conditions are intermittent stirring, the stirring speed is 800 to 1200 rpm, and the stirring is performed for 10 to 20 minutes, and then the mixture is allowed to stand for 6 to 10 minutes, and the mixture is cycled for 3 to 5 times. The mixture is then transferred to a high-speed disperser for dispersion, and the dispersion time is 1 to 2 hours to obtain an aqueous ceramic emulsion premix.
[0084] (3) Preparation of zinc phosphate emulsion premix:
[0085] 70 parts by mass of zinc phosphate emulsion, 0.2 parts by mass of defoamer, 0.2 parts by mass of leveling agent, 1.5 parts by mass of thickener and 28.1 parts by mass of water are mixed and stirred uniformly for 30 to 90 minutes at a stirring speed of 600 to 1000 rpm to obtain a zinc phosphate emulsion premix.
[0086] (4) Preparation of water-based room temperature curing ceramic coating:
[0087] 50 parts by mass of the aqueous ceramic emulsion premix obtained in (2) is added to 50 parts by mass of the zinc phosphate emulsion premix obtained in (3), and the mixture is mixed and ground for 0.5 to 1.5 hours, and the cooling water is adjusted so that the temperature of the ground material does not exceed 60° C. After the grinding is completed, the mixture is filtered to obtain a water-based room temperature curing ceramic coating.
[0088] Example 4
[0089] The preparation method of water-based room temperature curing ceramic coating comprises the following steps:
[0090] (1) Preparation of aqueous inorganic nano-ceramic emulsion:
[0091] The first step: adding 0.5 parts by mass of a surfactant to 30 parts by mass of dimethyldiethoxysilane and stirring evenly to obtain a pretreated organosilane; then dropping the pretreated organosilane into 42 parts by mass of silica sol, the titration time is 30 minutes, and then after the titration is completed, the temperature is raised to maintain the reaction temperature at 35-70°C, the constant temperature reaction is performed for 0.5-5 hours, and then a certain amount of water is added, the heating is stopped, and the temperature is lowered to obtain a water-based silane-modified nano-silicon emulsion;
[0092] Step 2: 0.2 parts by mass of surfactant and 80 parts by mass of water are mixed and mixed evenly to obtain a surfactant aqueous solution; then 28 parts by mass of aminosilane hydrolyzate is added dropwise to the pre-stirred surfactant aqueous solution for 30 minutes, and then the stirring reaction is continued for 0.5 to 2 hours, and then a certain amount of water is added, and the temperature is lowered to room temperature to obtain a pre-treated aqueous silicone dispersion;
[0093] Step 3: Mix all the aqueous silane-modified nano-silicon emulsion obtained in the first step with all the aqueous silicone dispersion obtained in the second step, and after mixing evenly, obtain an aqueous inorganic nano-ceramic emulsion.
[0094] (2) Preparation of aqueous ceramic emulsion premix:
[0095] 50 parts by mass of the aqueous inorganic nano-ceramic emulsion obtained in (1), 20 parts by mass of a filler, 10 parts by mass of a pigment, 0.5 parts by mass of a wetting and dispersing agent, and 19.5 parts by mass of water are placed in a grinder and ground for 0.5 to 1.5 hours, and then transferred to a stirring tank and stirred evenly. The stirring conditions are intermittent stirring, the stirring speed is 800 to 1200 rpm, and the stirring is performed for 10 to 20 minutes, and then the mixture is allowed to stand for 6 to 10 minutes, and the mixture is cycled for 3 to 5 times. The mixture is then transferred to a high-speed disperser for dispersion, and the dispersion time is 1 to 2 hours to obtain an aqueous ceramic emulsion premix.
[0096] (3) Preparation of zinc phosphate emulsion premix:
[0097] 75 parts by mass of zinc phosphate emulsion, 0.3 parts by mass of defoamer, 0.3 parts by mass of leveling agent, 1 part by mass of thickener and 23.4 parts by mass of water are mixed and stirred uniformly for 30 to 90 minutes at a stirring speed of 600 to 1000 rpm to obtain a zinc phosphate emulsion premix.
[0098] (4) Preparation of water-based room temperature curing ceramic coating:
[0099] 60 parts by mass of the aqueous ceramic emulsion premix obtained in (2) is added to 40 parts by mass of the zinc phosphate emulsion premix obtained in (3), and the mixture is mixed and ground for 0.5 to 1.5 hours, and the cooling water is adjusted so that the temperature of the ground material does not exceed 60° C. After the grinding is completed, the mixture is filtered to obtain a water-based room temperature curing ceramic coating.
[0100] Example 5
[0101] The preparation method of water-based room temperature curing ceramic coating comprises the following steps:
[0102] (1) Preparation of aqueous inorganic nano-ceramic emulsion:
[0103] The first step: adding 0.5 parts by mass of a surfactant to 35 parts by mass of methacryloxypropyltrimethoxysilane and stirring evenly to obtain a pretreated organosilane; then dropping the pretreated organosilane into 37 parts by mass of silica sol, the titration time is 30 minutes, and then after the titration is completed, the temperature is raised to maintain the reaction temperature at 35 to 70° C., the reaction is carried out at a constant temperature for 0.5 to 5 hours, and then a certain amount of water is added, the heating is stopped, and the temperature is lowered to obtain a water-based silane-modified nano-silicon emulsion;
[0104] Step 2: 0.2 parts by mass of surfactant and 80 parts by mass of water are mixed and mixed evenly to obtain a surfactant aqueous solution; then 28 parts by mass of aminosilane hydrolyzate is added dropwise to the pre-stirred surfactant aqueous solution for 30 minutes, and then the stirring reaction is continued for 0.5 to 2 hours, and then a certain amount of water is added, and the temperature is lowered to room temperature to obtain a pre-treated aqueous silicone dispersion;
[0105] Step 3: Mix all the aqueous silane-modified nano-silicon emulsion obtained in the first step with all the aqueous silicone dispersion obtained in the second step, and after mixing evenly, obtain an aqueous inorganic nano-ceramic emulsion.
[0106] (2) Preparation of aqueous ceramic emulsion premix:
[0107] 55 parts by mass of the aqueous inorganic nano-ceramic emulsion obtained in (1), 25 parts by mass of a filler, 10 parts by mass of a pigment, 0.5 parts by mass of a wetting and dispersing agent, and 9.5 parts by mass of water are placed in a grinder and ground for 0.5 to 1.5 hours, and then transferred to a stirring tank and stirred evenly. The stirring conditions are intermittent stirring, the stirring speed is 800 to 1200 rpm, and the stirring is performed for 10 to 20 minutes, and then the mixture is allowed to stand for 6 to 10 minutes, and the cycle is repeated 3 to 5 times. The mixture is then transferred to a high-speed disperser for dispersion, and the dispersion time is 1 to 2 hours to obtain an aqueous ceramic emulsion premix.
[0108] (3) Preparation of zinc phosphate emulsion premix:
[0109] 80 parts by mass of zinc phosphate emulsion, 0.15 parts by mass of defoamer, 0.2 parts by mass of leveling agent, 1 part by mass of thickener and 18.65 parts by mass of water are mixed and stirred uniformly for 30 to 90 minutes at a stirring speed of 600 to 1000 rpm to obtain a zinc phosphate emulsion premix.
[0110] (4) Preparation of water-based room temperature curing ceramic coating:
[0111] 70 parts by mass of the aqueous ceramic emulsion premix obtained in (2) is added to 30 parts by mass of the zinc phosphate emulsion premix obtained in (3), and the mixture is mixed and ground for 0.5 to 1.5 hours, and the cooling water is adjusted so that the temperature of the ground material does not exceed 60° C. After the grinding is completed, the mixture is filtered to obtain a water-based room temperature curing ceramic coating.
[0112] Example 6
[0113] The preparation method of water-based room temperature curing ceramic coating comprises the following steps:
[0114] (1) Preparation of aqueous inorganic nano-ceramic emulsion:
[0115] The first step: adding 0.5 parts by mass of a surfactant to 42 parts by mass of methacryloxypropyltrimethoxysilane and stirring evenly to obtain a pretreated organosilane; then dropping the pretreated organosilane into 33 parts by mass of silica sol, the titration time is 30 minutes, and then after the titration is completed, the temperature is raised to maintain the reaction temperature at 35-70°C, the constant temperature reaction is performed for 0.5-5 hours, and then a certain amount of water is added, the heating is stopped, and the temperature is lowered to obtain a water-based silane-modified nano-silicon emulsion;
[0116] Step 2: 0.2 parts by mass of surfactant and 80 parts by mass of water are mixed and mixed evenly to obtain a surfactant aqueous solution; then 25 parts by mass of aminosilane hydrolyzate is added dropwise to the pre-stirred surfactant aqueous solution for 30 minutes, and then the stirring reaction is continued for 0.5 to 2 hours, and then a certain amount of water is added, and the temperature is lowered to room temperature to obtain a pre-treated aqueous silicone dispersion;
[0117] Step 3: Mix all the aqueous silane-modified nano-silicon emulsion obtained in the first step with all the aqueous silicone dispersion obtained in the second step, and after mixing evenly, obtain an aqueous inorganic nano-ceramic emulsion.
[0118] (2) Preparation of aqueous ceramic emulsion premix:
[0119] 60 parts by mass of the aqueous inorganic nano-ceramic emulsion obtained in (1), 25 parts by mass of a filler, 10 parts by mass of a pigment, 0.3 parts by mass of a wetting and dispersing agent, and 4.7 parts by mass of water are placed in a grinder and ground for 0.5 to 1.5 hours, and then transferred to a stirring tank and stirred evenly. The stirring conditions are intermittent stirring, the stirring speed is 800 to 1200 rpm, and the stirring is performed for 10 to 20 minutes, and then the mixture is allowed to stand for 6 to 10 minutes, and the mixture is cycled for 3 to 5 times. The mixture is then transferred to a high-speed disperser for dispersion, and the dispersion time is 1 to 2 hours to obtain an aqueous ceramic emulsion premix.
[0120] (3) Preparation of zinc phosphate emulsion premix:
[0121] 85 parts by mass of zinc phosphate emulsion, 0.2 parts by mass of defoamer, 0.3 parts by mass of leveling agent, 0.2 parts by mass of thickener and 14.3 parts by mass of water are mixed and stirred uniformly for 30 to 90 minutes at a stirring speed of 600 to 1000 rpm to obtain a zinc phosphate emulsion premix.
[0122] (4) Preparation of water-based room temperature curing ceramic coating:
[0123] 80 parts by mass of the aqueous ceramic emulsion premix obtained in (2) is added to 20 parts by mass of the zinc phosphate emulsion premix obtained in (3), and the mixture is mixed and ground for 0.5 to 1.5 hours, and the cooling water is adjusted so that the temperature of the ground material does not exceed 60° C. After the grinding is completed, the mixture is filtered to obtain a water-based room temperature curing ceramic coating.
[0124] Table 1 Mass percentage of raw materials for preparing aqueous inorganic nano-ceramic emulsion (%)
[0125]
[0126] Table 2 Mass percentage of raw materials for preparing aqueous ceramic emulsion premix (%)
[0127]
[0128]
[0129] Table 3 Mass percentage of raw materials for preparing zinc phosphate emulsion premix (%)
[0130]
[0131] Table 4 Mass percentage of raw materials for preparing water-based room temperature curing nano ceramic coatings (%)
[0132]
[0133] Table 5 Performance indexes of room temperature curing ceramic coatings
[0134]
[0135] The water-based room-temperature curing ceramic coating prepared by the invention has the properties of high hardness, high wear resistance, waterproofness, super weather resistance and the like.
[0136] The water-based room-temperature curing ceramic coating provided by the present invention has the advantages of strong durability, high hardness, strong adhesion to cement-based materials and room-temperature curing compared to the products in the prior art. It can provide decoration, waterproofing, protection, repair and other functions for cement-based materials.
[0137] The above embodiments are only provided as demonstrations under the technical principle of the present invention, and are not intended to limit the present invention. Any person familiar with the present technology may adjust or improve the above embodiments without violating the principle and scope of the present invention. All equivalent modifications or changes made by those with ordinary knowledge in the relevant technical field without departing from the technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A water-based room temperature curing ceramic coating, characterized in that: The following raw materials are included in mass percentage: Water-based inorganic nano-ceramic emulsion premix 30-80% Zinc phosphate emulsion premix 20-70%.
2. The water-based room temperature curing ceramic coating according to claim 1, characterized in that: The aqueous inorganic nano-ceramic emulsion premix comprises the following raw materials in percentage by mass:
3. The water-based room temperature curing ceramic coating according to claim 1, characterized in that: The zinc phosphate emulsion premix comprises the following raw materials in percentage by weight:
4. The water-based room temperature curing ceramic coating according to claim 2, characterized in that: The aqueous inorganic nano-ceramic emulsion comprises the following raw materials in percentage by mass: Silica sol 33~55% Organosilane 12~42% Aqueous silicone dispersion 25-33%.
5. The water-based room temperature curing ceramic coating according to claim 4, characterized in that: The silica sol is acidic silica sol, alkaline silica sol or a mixture of the two; The organosilane is selected from the group consisting of methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, 3-glycidyloxypropyltrimethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, glycidoxypropylmethyldimethoxysilane, glycidoxypropylmethyldiethoxysilane, diphenyldimethoxysilane, and a mixture of two or more thereof; The aqueous organosilicon dispersion adopts aminosilane hydrolyzate.
6. The water-based room temperature curing ceramic coating according to claim 4, characterized in that: The organosilane and aqueous organosilicon dispersion are pretreated with a surfactant.
7. The water-based room temperature curing ceramic coating according to claim 6, characterized in that: The surfactant is one of carboxylate type, sulfonate type, citrate type, sulfate (ester) salt type and phosphate (ester) salt type or a mixture of two or more of them.
8. The water-based room temperature curing ceramic coating according to claim 2, characterized in that: The filler is one or a mixture of two or more of mica powder, nano-fumed silica, kaolin, whisker silicon, micron- and nano-sized spherical alumina, calcium sulfate whisker, magnesium sulfate whisker, aluminum borate whisker and zirconium sulfate whisker; The pigment is one or a mixture of two or more of titanium dioxide, copper chrome black, cobalt black, manganese iron black, pearlescent pigment, fluorescent pigment and metallic pigment; The wetting and dispersing agent is BASF dispersant Dispex Ultra PX 4575.
9. The water-based room temperature curing ceramic coating according to claim 3, characterized in that: The zinc phosphate emulsion is prepared by the steps of reaction, aging, washing, filtering and emulsification of phosphate and zinc salt; The defoamer is silicone defoamer S771; The leveling agent is methyl silicone oil, hydroxy silicone oil or a mixture of the two; The thickener is a special thickener for emulsified silicone oil.
10. The method for preparing a water-based room temperature curing ceramic coating according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Preparation of aqueous inorganic nano-ceramic emulsion: The first step: adding a surfactant to the organosilane and stirring evenly to obtain a pretreated organosilane; then dropping the pretreated organosilane into the silica sol, the titration time is 30 minutes, and after the titration is completed, the temperature is raised to maintain the reaction temperature at 35-70°C, and the reaction is carried out at a constant temperature for 0.5-5 hours, and then a certain amount of water is added, the heating is stopped, and the temperature is lowered to obtain a water-based silane-modified nano-silicon emulsion; Step 2: Mix the surfactant and water to obtain a surfactant aqueous solution; then drop the aminosilane hydrolyzate into the pre-mixed surfactant aqueous solution for 30 minutes, and then continue to stir and react for 0.5 to 2 hours, then add a certain amount of water, and cool to room temperature to obtain a pre-treated aqueous silicone dispersion; Step 3: Mix the water-based silane-modified nano-silicon emulsion obtained in the first step with the water-based organosilicon dispersion obtained in the second step in a certain proportion, and after mixing evenly, obtain a water-based inorganic nano-ceramic emulsion; (2) Preparation of aqueous ceramic emulsion premix: The aqueous inorganic nano-ceramic emulsion obtained in (1), as well as the filler, pigment, wetting dispersant and water are placed in a grinder and ground for 0.5 to 1.5 hours, and then transferred to a stirring tank and stirred evenly. The stirring conditions are intermittent stirring, the stirring speed is 800 to 1200 rpm, and each stirring is 10 to 20 minutes, and then the mixture is allowed to stand for 6 to 10 minutes, and the cycle is repeated 3 to 5 times. The mixture is then transferred to a high-speed disperser for dispersion, and the dispersion time is 1 to 2 hours to obtain an aqueous ceramic emulsion premix; (3) Preparation of zinc phosphate emulsion premix: Mix zinc phosphate emulsion, defoamer, leveling agent, thickener and water and stir evenly for 30 to 90 minutes at a stirring speed of 600 to 1000 rpm to obtain a zinc phosphate emulsion premix: (4) Preparation of water-based room temperature curing ceramic coating: The water-based ceramic emulsion premix obtained in (2) is added to the zinc phosphate emulsion premix obtained in (3) and mixed and ground for 0.5 to 1.5 hours, and the cooling water is adjusted so that the temperature of the ground material does not exceed 60° C. After the grinding is completed, it is filtered to obtain a water-based room temperature curing ceramic coating.
Citation Information
Patent Citations
Normal temperature cured super weather-resistant and wear-resistant high-hardness water-based inorganic nanoceramic coating and preparation method thereof
CN109266057A
Room temperature curable ceramic coating composition
KR1020180085135A