Adhesive tape with high adhesive force, preparation method and application

By designing a specific tape structure and an interpenetrating network structure, the problem of insufficient adhesion of high-temperature tapes at high temperatures has been solved, achieving stable adhesion and wide applicability in high-temperature environments.

CN118956288APending Publication Date: 2024-11-15ANHUI MINGXUN NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411065811.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing high-temperature resistant tapes have short bonding times under high-temperature conditions, making it difficult to bond low-energy surface materials. They are also prone to delamination at temperatures exceeding 180°C, resulting in a small bonding range.

Method used

The tape structure consists of a transparent release layer, silicone pressure-sensitive adhesive, a substrate layer, acrylic pressure-sensitive adhesive, and a white release layer. The acrylic pressure-sensitive adhesive is composed of specific monomers and forms an interpenetrating network structure through a cross-linking reaction, which enhances the bonding performance.

Benefits of technology

It maintains excellent adhesion at high temperatures of 175-220℃, does not yellow or foam, is suitable for a variety of backing materials, and is widely used in materials such as aluminum foil, glass, and leather.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004979323200000051
    Figure BDA0004979323200000051
  • Figure BDA0004979323200000062
    Figure BDA0004979323200000062
Patent Text Reader

Abstract

The invention provides a high-adhesion adhesive tape as well as a preparation method and application thereof. The adhesive tape sequentially comprises a transparent release layer, a silica gel pressure-sensitive adhesive, a base material layer, an acrylic acid pressure-sensitive adhesive and a white release layer from top to bottom, and is characterized in that synthetic monomers of the acrylic acid pressure-sensitive adhesive comprise isobutyl acrylate, vinyl acetate, oleylamine, butyric acid and ethylene glycol. By adjusting the proportion of various monomers in the raw materials of the shell material and the core material, the acrylic pressure-sensitive adhesive shows soft hand feeling and outstanding elasticity, the mechanical stability of the acrylic pressure-sensitive adhesive at different temperatures is improved, an interpenetrating network structure is formed, various backboard materials can be well bonded, yellowing and foaming are avoided, and the application range is wide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer functional materials, and in particular to a high-adhesion adhesive tape, a preparation method and application thereof. Background Art

[0002] With the rapid improvement of social economy and people's living standards, adhesive tapes have been fully integrated into all walks of life and people's daily life. Adhesive tapes are not only widely used, but also of many types, such as: high temperature resistant tapes used in high temperature working environments; this type of tape is mainly used in the electronics industry, and its temperature resistance is usually between 120 degrees and 260 degrees. It is often used in spray painting, baking varnish leather processing, coating masking, fixing in electronic parts manufacturing processes, printed circuit boards, and high temperature processing masking.

[0003] At present, there are many problems with the substrates and adhesives used in high temperature resistant tapes, such as: the substrates are mostly single-layer traditional materials with average heat resistance and wear resistance; the adhesives are mostly acrylic pressure-sensitive adhesives, which have excellent bonding properties, chemical stability, and advantages such as non-toxicity, harmlessness, and low cost, but have average heat resistance. At higher temperatures, they have poor heat-oxidative aging resistance and are prone to losing pressure sensitivity. Even cross-linked acrylic pressure-sensitive adhesives can only be used for a short period of time at 150°C. In current technologies, high-performance high temperature resistant tapes that can simultaneously have high peel strength, high initial adhesion, and a wide range of operating temperatures are rare, especially high temperature resistant tapes that can withstand extremely high temperatures when used for a short period of time.

[0004] Patent CN107236490A discloses a method for preparing a high temperature resistant pressure sensitive adhesive, wherein a silicone gel rich in silanol is prepared by a hydrochloric acid decomposition method, and then a zeolite is treated with a silicate to make the zeolite surface have silanol, and then concentrated sulfuric acid is used as a catalyst to make the silicone gel and the silanol on the surface of the zeolite undergo a dehydration condensation reaction to form a Si-O-Si bond with extremely high bond energy. Since the bond energy of the Si-O-Si bond is greater than that of the CC bond and the CO bond in general organic matter, it has good high temperature resistance, and then a natural resin is used to modify the filler under the action of microorganisms to increase the number of natural resin particles on the filler surface and improve the compatibility between the high temperature resistant filler and the acrylate. Although the high temperature resistant pressure sensitive adhesive in the technical solution has good high temperature stability, it can only maintain adhesion for 30-33 minutes without degumming at 175-180°C, and the viscosity is 2550-2620mPa·s; if the temperature continues to rise to 220°C, problems such as foaming, severe yellowing, molecular chain cleavage and loss of pressure sensitivity will occur. Summary of the invention

[0005] Purpose of the invention: The purpose of the present invention is to provide a high-adhesion tape, preparation method and application to address the defects of current acrylic pressure-sensitive adhesives, such as short bonding time under high temperature conditions, difficulty in bonding low-energy surface materials, small bonding range, and easy debonding under high temperature environments exceeding 180°C.

[0006] The technical solution of the present invention:

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0008] On the one hand, the present invention provides a high-adhesion tape; the tape comprises, from top to bottom, a transparent release layer, a silicone pressure-sensitive adhesive, a substrate layer, an acrylic pressure-sensitive adhesive and a white release layer, characterized in that the synthetic monomers of the acrylic pressure-sensitive adhesive comprise isobutyl acrylate, vinyl acetate, oleylamine, butyric acid and ethylene glycol.

[0009] In some embodiments, the acrylic pressure-sensitive adhesive is divided into a core material and a shell material, the monomers for preparing the core material include isobutyl acrylate and vinyl acetate, and the monomers for preparing the shell material include isobutyl acrylate, vinyl acetate, oleylamine, butyric acid and ethylene glycol.

[0010] In some embodiments, the method for preparing the acrylic pressure-sensitive adhesive comprises:

[0011] Step 1: Add distilled water and an emulsifier into a reactor, add isobutyl acrylate and vinyl acetate, and stir evenly to prepare a core material emulsion;

[0012] Step 2: Ethylene glycol is substituted with hydrogen chloride under anhydrous conditions to obtain chloroethylene glycol, chloroethylene glycol is esterified with butyrate to obtain chloroethylene butyrate, and chloroethylene butyrate is reacted with oleylamine to obtain a crosslinking monomer;

[0013] Step 3: Add distilled water and an emulsifier into a reactor, add isobutyl acrylate, vinyl acetate and a cross-linking monomer, and stir evenly to prepare a shell material emulsion;

[0014] Step 4: Add a mixed solution of distilled water and polyvinyl alcohol into a reactor, then add an emulsifier, drop an initiator and a core material emulsion, and heat the reaction; continue to drop the shell material emulsion and the initiator, and after the dropwise addition is completed, heat the reaction and discharge the material to obtain an acrylic pressure-sensitive adhesive.

[0015] In some embodiments, the emulsifier can be selected from Tween series emulsifiers or Span series emulsifiers; for example, one or more combinations of Tween60, Tween65, Tween80, Span65, and Span80 can be selected as emulsifiers, which are suitable for the preparation of water / oil emulsions.

[0016] In some embodiments, the initiator is selected from one or more combinations of persulfate initiators, bisulfite initiators, chlorate initiators, etc. For example, one or more combinations of sodium bisulfite, ammonium persulfate, potassium persulfate, and sodium persulfate can be selected as initiators to initiate free radical polymerization and oxidation reactions.

[0017] In some embodiments, in step 1, the molar ratio of isobutyl acrylate to vinyl acetate is 1:2.5-4; preferably, the molar ratio of isobutyl acrylate to vinyl acetate is 1:3.

[0018] In some embodiments, in step 3, the molar ratio of isobutyl acrylate, vinyl acetate and cross-linking monomer is 1:1-2.5:0.05-0.3; preferably, the molar ratio of isobutyl acrylate, vinyl acetate and cross-linking monomer is 1:2:0.2.

[0019] In some embodiments, in step 4, the volume ratio of the core material emulsion to the shell material emulsion is 1:1.2-1.5.

[0020] Adjusting the ratio of various monomers in the shell material and core material raw materials can make the acrylic pressure-sensitive adhesive present a soft feel and outstanding elasticity. At the same time, the addition of isobutyl acrylate introduces carboxyl groups, which creates spatial barriers and increases the mechanical stability of the acrylic pressure-sensitive adhesive at different temperatures. The addition of cross-linking monomers can bond the structures on the shell material and core material through the double bonds on the monomers, further cross-linking and curing the adhesive layer to form an interpenetrating network structure.

[0021] In some embodiments, the transparent release layer is a PET silicone release film.

[0022] In some embodiments, the silicone pressure-sensitive adhesive is a silicone resin adhesive. The type of silicone pressure-sensitive adhesive is not limited in the present invention. For example, DET-1100 silicone pressure-sensitive adhesive can be used.

[0023] In some embodiments, the material of the substrate layer is any one of PET, PI, PC, and PU, and PET is generally selected as the substrate.

[0024] In some embodiments, the white release layer is a PET white release film.

[0025] In some embodiments, the thicknesses of the transparent release layer, the silicone pressure-sensitive adhesive, the substrate layer, the acrylic pressure-sensitive adhesive and the white release layer are 50±2 μm, 100±10 μm, 25±2 μm, 100±10 μm and 25±2 μm, respectively.

[0026] In another aspect, the present invention also provides a method for preparing the adhesive tape:

[0027] Step 1: Evenly apply acrylic pressure-sensitive adhesive and silicone pressure-sensitive adhesive on the upper and lower surfaces of the substrate layer, respectively, and place at 80-150° C. for heat preservation and curing for 1-20 minutes to form a pressure-sensitive adhesive layer;

[0028] Step 2: Place the transparent coated release film and the white release film on the outside of the acrylic pressure-sensitive adhesive and the silicone pressure-sensitive adhesive in step 1 respectively, place them at 80-150°C for drying and curing for 1-10 minutes to form a release layer, and then roll and cut them to obtain a tape.

[0029] In another aspect, the present invention also provides use of the adhesive tape on aluminum foil, glass or leather.

[0030] In some embodiments, the adhesive tape is used in an environment with a temperature of 175-220°C.

[0031] The adhesive tape of the present invention has excellent initial adhesion performance, and has excellent adhesion under high temperature conditions of 175-180°C, even at 220°C, without yellowing or foaming, and is also suitable for a variety of backing materials; in view of this, the adhesive tape provided by the present invention has a wide range of applications and is suitable for popularization and use.

[0032] Beneficial effects:

[0033] The high-adhesion adhesive tape provided by the present invention can still maintain excellent adhesion in a high-temperature environment exceeding 180° C., can achieve good adhesion to various backplane materials, does not turn yellow or foam, and has a wide range of applications. DETAILED DESCRIPTION

[0034] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0035] Unless otherwise specified, the chemical reagents used in the present invention are all commercially available analytically pure.

[0036] Preparation of acrylic pressure-sensitive adhesive 1

[0037] Step 1: Add 50 ml of distilled water and 2 mol of emulsifier Tween80 into a reactor, add 2 mol of isobutyl acrylate and 5 mol of vinyl acetate under stirring, and stir evenly to prepare a core material emulsion;

[0038] Step 2: Add 1 mol of ethylene glycol, 0.5 mol of hydrogen chloride and 20 ml of toluene to a reactor, heat at 40°C for 1 hour to react, perform a substitution reaction, extract and dry to obtain chloroethylene glycol; then add 1 mol of chloroethylene glycol and 1 mol of butyric acid to the reactor, add 0.03 mol of concentrated sulfuric acid, heat at 100°C for esterification, extract and recrystallize to obtain chloroethylene butyrate; then take 1.2 mol of oleylamine and add it to 50 ml of DMF solvent, slowly drop 1 mol of chloroethylene butyrate, and react at a constant temperature of 30°C to obtain a cross-linking monomer;

[0039] Mass spectrometry data for testing cross-linked monomers: The obtained products were analyzed by LC-MS, and the m / z of the products were 381.36 (100.0%), 382.38 (27.3%), and 383.38 (3.7%), confirming that ethylene glycol, butyric acid, and oleylamine were successfully bonded to obtain the desired structure;

[0040] Step 3: Add 50 ml of distilled water and 1 mol of emulsifier, 2 mol of isobutyl acrylate, 2 mol of vinyl acetate and 0.1 mol of cross-linking monomer into the reactor, and stir evenly to prepare a shell material emulsion;

[0041] Step 4: Add a mixed solution of 30 ml of distilled water and 30 ml of polyvinyl alcohol into the reactor, then add 2 mol of emulsifier, drop 0.5 mol of initiator sodium persulfate and 20 ml of the core material emulsion prepared in step 1, heat to 75°C and react for 1.5 hours; continue to drop 24 ml of the shell material emulsion prepared in step 3 and 0.3 mol of initiator sodium persulfate, maintain 75°C for 2 hours after the addition is completed, cool to room temperature after the reaction is completed, and discharge to obtain acrylic pressure-sensitive adhesive 1.

[0042] Preparation of acrylic pressure-sensitive adhesive 2

[0043] The preparation method of acrylic pressure-sensitive adhesive 2 refers to that of acrylic pressure-sensitive adhesive 1, except that in step 1, the added molar amounts of isobutyl acrylate and vinyl acetate are 2 mol and 8 mol, respectively; in step 3, the added molar amounts of isobutyl acrylate and the cross-linking monomer are 2 mol, 5 mol and 0.6 mol, respectively.

[0044] Preparation of acrylic pressure-sensitive adhesive 3

[0045] The preparation method of acrylic pressure-sensitive adhesive 3 refers to that of acrylic pressure-sensitive adhesive 1, except that in step 1, the added molar amounts of isobutyl acrylate and vinyl acetate are 2 mol and 6 mol, respectively; in step 3, the added molar amounts of isobutyl acrylate and the cross-linking monomer are 2 mol, 4 mol and 0.4 mol, respectively.

[0046] Preparation of acrylic pressure-sensitive adhesive 4

[0047] The preparation method of acrylic pressure-sensitive adhesive 4 is similar to that of acrylic pressure-sensitive adhesive 1, except that in step 3, the added molar amounts of isobutyl acrylate, vinyl acetate and cross-linking monomer are 2 mol, 8 mol and 0.6 mol respectively.

[0048] Preparation of acrylic pressure-sensitive adhesive 5

[0049] The preparation method of acrylic pressure-sensitive adhesive 5 is similar to that of acrylic pressure-sensitive adhesive 1, except that in step 3, the added molar amounts of isobutyl acrylate, vinyl acetate and cross-linking monomer are 2 mol, 2 mol and 0 mol respectively.

[0050] Preparation of acrylic pressure-sensitive adhesive 6

[0051] The preparation method of acrylic pressure-sensitive adhesive 6 is as follows:

[0052] Step 1: Add 1 mol of ethylene glycol, 0.5 mol of hydrogen chloride and 20 ml of toluene to a reactor, heat at 40°C for 1 hour to react, perform a substitution reaction, extract and dry to obtain chloroethylene glycol; then add 1 mol of chloroethylene glycol and 1 mol of butyric acid to the reactor, add 0.03 mol of concentrated sulfuric acid, heat at 100°C for esterification, extract and recrystallize to obtain chloroethylene butyrate; then take 1.2 mol of oleylamine and add it to 50 ml of DMF solvent, slowly drop 1 mol of chloroethylene butyrate, and react at a constant temperature of 30°C to obtain a cross-linking monomer;

[0053] Step 2: 4 mol of isobutyl acrylate, 7 mol of vinyl acetate, 0.1 mol of crosslinking monomer, 100 ml of distilled water and 5 mol of emulsifier were added to a reaction vessel and heated to 75° C. while stirring;

[0054] Step 3: Add 0.8 mol of initiator to a mixed solution of 30 ml of distilled water and 30 ml of polyvinyl alcohol and mix well, then drop the mixture into the reaction vessel of step 3 at a uniform speed, stir during the dropwise addition and keep the temperature at 75°C, and react for 2 hours;

[0055] Step 4: Cool to room temperature, discharge the material, and obtain acrylic pressure-sensitive adhesive 6.

[0056] Examples and Comparative Examples

[0057] Step 1: Evenly coat the upper and lower surfaces of the substrate layer (PET, Dongguan Tianyi Chemical Co., Ltd.) with acrylic pressure-sensitive adhesive and silicone pressure-sensitive adhesive (DET-1100), respectively, and place at 80-150° C. for curing for 1-20 minutes to form a pressure-sensitive adhesive layer;

[0058] Step 2: Place the transparent coated release film (JT-561) and the white release film (JT-408) on the outside of the acrylic pressure-sensitive adhesive and the silicone pressure-sensitive adhesive in step 1, respectively, place them at 80-150°C for drying and curing for 1-10 minutes, and then roll and cut them to obtain the product.

[0059] The thicknesses of the transparent release layer, the silicone pressure-sensitive adhesive, the substrate layer, the acrylic pressure-sensitive adhesive and the white release layer are 50 μm, 110 μm, 25 μm, 110 μm and 25 μm, respectively.

[0060] Table 1 Types of acrylic pressure-sensitive adhesives used in Examples and Comparative Examples

[0061]

[0062]

[0063] Performance Testing

[0064] The following performance tests were performed on the above adhesive tapes 1-7:

[0065] Peel strength test: The white release film of the above tapes was torn off, and the tapes were adhered to the backing materials (aluminum foil, glass and leather) using a pressure of 4 bar. The samples were first cured at 110°C for 3 minutes, and then placed in a 50°C oven for further aging for 48 hours. After that, a 180° peel strength test was performed at 90°C. The adhesion test conditions were 220°C and 85% relative humidity. The test results are shown in Table 2.

[0066] Table 2 Test results of tapes 1-7

[0067]

[0068] As can be seen from the table above, the high-adhesion adhesive tape of the present invention adopts an acrylic pressure-sensitive adhesive with an interpenetrating network structure core-shell structure, and the 180° peeling force test of various backing materials can be maintained between 17-30N / 25mm, and the adhesive force can be maintained for 72h at 220°C and 85% humidity. After the test, the adhesive tape is torn without debonding. This shows that the product provided by the present invention can be applied to various backing materials and has strong universality.

[0069] It can be seen from the table that the addition of cross-linking monomers can further cross-link and solidify the adhesive layer through the double bonds on the monomers to bond the shell material and the core material, forming an interpenetrating network structure. The interpenetrating network structure can enhance the viscosity and toughness of the acrylic pressure-sensitive adhesive, reduce the generation of residual adhesive or even leave no residual adhesive when peeling, and provide customers with a comfortable use experience.

[0070] When preparing the shell material and the core material, selecting different monomer ratios will affect the viscosity and toughness of the acrylic pressure-sensitive adhesive actually obtained. Adjusting the monomer ratio to the parameters of Example 3 can achieve better peel strength and adhesion time.

[0071] The present invention can also have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.

Claims

1. A high-adhesion tape, comprising, from top to bottom, a transparent release layer, a silicone pressure-sensitive adhesive, a substrate layer, an acrylic pressure-sensitive adhesive and a white release layer; characterized in that: The synthetic monomers of the acrylic pressure-sensitive adhesive include isobutyl acrylate, vinyl acetate, oleylamine, butyric acid and ethylene glycol.

2. The high-adhesion adhesive tape according to claim 1, characterized in that: The acrylic pressure-sensitive adhesive is divided into a core material and a shell material; the monomers for preparing the core material include isobutyl acrylate and vinyl acetate, and the monomers for preparing the shell material include isobutyl acrylate, vinyl acetate, oleylamine, butyric acid and ethylene glycol.

3. The high-adhesion adhesive tape according to claim 1, characterized in that: The preparation method of the acrylic pressure-sensitive adhesive comprises: Step 1: Add distilled water and an emulsifier into a reactor, add isobutyl acrylate and vinyl acetate, and stir evenly to prepare a core material emulsion; Step 2: Ethylene glycol is substituted with hydrogen chloride under anhydrous conditions to obtain chloroethylene glycol, chloroethylene glycol is esterified with butyrate to obtain chloroethylene butyrate, and chloroethylene butyrate is reacted with oleylamine to obtain a crosslinking monomer; Step 3: Add distilled water and an emulsifier into a reactor, add isobutyl acrylate, vinyl acetate and a cross-linking monomer, and stir evenly to prepare a shell material emulsion; Step 4: Add a mixed solution of distilled water and polyvinyl alcohol into a reactor, then add an emulsifier, drop an initiator and a core material emulsion, and heat the reaction; continue to drop the shell material emulsion and the initiator, and after the dropwise addition is completed, heat the reaction and discharge the material to obtain an acrylic pressure-sensitive adhesive.

4. The high-adhesion adhesive tape according to claim 3, characterized in that: In the step 1, the molar ratio of isobutyl acrylate to vinyl acetate is 1:2.5-4.

5. The high-adhesion adhesive tape according to claim 3, characterized in that: In the step 3, the molar ratio of isobutyl acrylate, vinyl acetate and cross-linking monomer is 1:1-2.5:0.05-0.

3.

6. The high-adhesion adhesive tape according to claim 3, characterized in that: In step 4, the volume ratio of the core material emulsion to the shell material emulsion is 1:1.2-1.

5.

7. The high-adhesion adhesive tape according to claim 1, characterized in that: The thicknesses of the transparent release layer, the silicone pressure-sensitive adhesive, the substrate layer, the acrylic pressure-sensitive adhesive and the white release layer are 50±2 μm, 100±10 μm, 25±2 μm, 100±10 μm and 25±2 μm, respectively.

8. The method for preparing the high-adhesion adhesive tape according to any one of claims 1 to 7, characterized in that: include: Step 1: Evenly apply acrylic pressure-sensitive adhesive and silicone pressure-sensitive adhesive on the upper and lower surfaces of the substrate layer, respectively, and place at 80-150° C. for heat preservation and curing for 1-20 minutes to form a pressure-sensitive adhesive layer; Step 2: Place the transparent coated release film and the white release film on the outside of the acrylic pressure-sensitive adhesive and the silicone pressure-sensitive adhesive in step 1 respectively, place them at 80-150° C. for drying and curing for 1-10 minutes to form a release layer, and then roll and cut them to obtain the tape.

9. Use of the high-adhesion tape according to any one of claims 1 to 7 on aluminum foil, glass or leather.

10. The use of the high-adhesion tape according to claim 8, characterized in that: The ambient temperature of the application is 175-220°C.