Foam-based phase-change composite material for night desert thermal insulation tent and preparation method of foam-based phase-change composite material
By adhering MoS2 nanoparticles to the porous foam skeleton and combining heat storage phase change materials, a multifunctional phase change composite material was prepared, which solved the problems of leakage and single function of traditional phase change materials, and achieved effective temperature regulation in desert areas and thermal energy storage and release, improving application flexibility and efficiency.
Patent Information
- Application Number
- CN202411020116.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional solid-liquid phase change materials are prone to liquid phase leakage above the melting point, resulting in low stability and difficulty in assembly, limiting their large-scale application, and a single function cannot meet the needs of diversified application, especially in the large environment of day and night temperature difference in desert areas. Effectively adjust the temperature.
MoS2 nanoparticles are adhered to the porous foam skeleton through PDMS and combined with the heat storage phase change material to prepare a multifunctional phase change composite material, which has the ability of phase change heat storage, temperature regulation and photothermal conversion, and through photothermal conversion Store heat energy during the day and release it at night to achieve insulation effect.
It solves the leakage problem of traditional phase change materials, provides composite materials that are easy to cut and control, has efficient photothermal conversion capabilities, can effectively adjust temperature in desert areas, improves application flexibility and efficiency, and realizes day and night temperature difference ease.
Smart Images

Figure CN118956352A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a foam-based phase-change composite material for a nighttime desert heat-insulating tent and a preparation method thereof, and particularly relates to the field of phase-change energy storage. Background Art
[0002] Thermal energy, as an energy source, is one of the main forms of energy dissipation, so the development of efficient thermal energy storage technology is crucial for energy conservation. The latent heat energy storage technology of phase change materials (PCMs) has the advantages of large energy storage capacity, stable temperature during phase change, and high safety. Therefore, PCMs have received extensive attention in many fields such as waste heat collection and utilization, intelligent temperature management, building energy conservation, and military.
[0003] Solid-liquid phase change materials have high latent heat and small volume change during phase change; they are the most commonly used PCMs. However, above the melting point, they will leak out of the liquid phase, resulting in low stability and difficulty in assembly, which greatly limits their large-scale application. Therefore, in the past decade, research on PCMs has focused on encapsulation technology. Based on a large number of previous studies, strategies for leak-proof PCMs have been developed, such as porous scaffold encapsulation and microencapsulation. Although the leakage problem has been solved, the single function of traditional PCMs can no longer meet people's needs. In order to meet the diverse application needs, multifunctional composite phase change materials must be developed. The application of functional fillers or carriers, such as graphene nanosheets, reduced graphene oxide, metal nanowires, and carbon aerogels, is an effective strategy to enrich the functions of PCMs. Studies have shown that the functions of phase change composites are closely related to the properties of the additives. Therefore, designing multifunctional fillers or scaffolds is one of the directions for the development of phase change composites.
[0004] Compared with core-shell microcapsules, core-shell materials have certain defects, such as weak thermal response of organic polymers, brittleness and poor compatibility with inorganic matrices, which limit the widespread application of the core-shell method. The adsorption of PCMs by porous materials mainly relies on the adsorption of their nano- and micron-sized pores. Compared with microcapsules, porous materials can adsorb more PCMs, have higher thermal energy utilization of PCMs, and have a simple preparation process. Porous foams have a highly open three-dimensional porous structure and great flexibility, making them excellent templates for constructing multifunctional scaffolds. Therefore, porous materials, as an ideal matrix, have aroused the research interest of scholars in many fields such as solar steam generators, batteries, sensors, and supercapacitors.
[0005] With the continuous development of science and technology, people gradually realize that desert areas have great development potential. However, due to the lack of water and the large temperature difference between day and night in desert areas, humans cannot live in them for a long time. Therefore, it is very meaningful to develop a material that can regulate temperature in the desert to solve the problem of hot deserts during the day and cold deserts at night, and phase change materials are a very good choice. Combining phase change materials with melamine foam can solve the leakage problem, but pure phase change materials do not have the ability of photothermal conversion, which limits the application of phase change materials in the intersection of photothermal conversion and energy storage. Therefore, it is of great significance to use natural sunlight to develop a phase change composite material that can be combined with tents and can use photothermal conversion for temperature regulation. When the outside temperature rises to the melting point of PCMs, PCMs gradually change from solid to liquid, absorb the heat from the outside and store it as latent heat. At this time, the microclimate in the tent remains unchanged at the phase change temperature point, which can alleviate the heat during the day; when the outside temperature drops, PCMs gradually solidify and release latent heat, and the microclimate temperature in the tent remains constant, which can alleviate the cold at night. The foam-based phase-change composite material for the nighttime desert thermal insulation tent developed by the present invention can significantly improve the physical sensation and comfort of humans in related activities in desert areas. Summary of the invention
[0006] In order to solve the above problems, the present invention adheres MoS2 nanoparticles to the MF skeleton through PDMS, and combines them with heat storage phase change materials to prepare a multifunctional phase change composite material, giving it the capabilities of phase change heat storage, temperature control and photothermal conversion.
[0007] Molybdenum disulfide (MoS2), which sandwiches a layer of Mo atoms between two layers of S atoms, has attracted much attention in the field of photothermal conversion due to its intrinsic band gap and unique layered structure as well as its broad visible and near-infrared absorption capabilities. Recent groundbreaking reports also show that MoS2 can greatly promote photothermal conversion due to its intrinsic charge and ultrathin thickness. MoS2-based composites have received unprecedented attention in energy conversion and storage due to their high thermal energy collection and release efficiency and good photothermal conversion properties.
[0008] According to the Stefan-Boltzmann law, the infrared radiation of an object is closely related to its surface temperature. Therefore, controlling the surface temperature of an object to be close to the ambient temperature can achieve infrared invisibility, or controlling the surface temperature of an object to achieve a false indication effect. Phase change materials can reach a stable temperature within a certain period of time, thereby achieving infrared invisibility and false indication.
[0009] The present invention solves the leakage problem of traditional solid-liquid phase change materials and provides a phase change composite material that is easy to cut and easy to control in size. The type and adsorption amount of solid-liquid phase change materials can be flexibly controlled, and the material has good photothermal conversion capability, which increases more application scenarios. The present invention can be applied in the fields of temperature control, photothermal conversion, infrared stealth, and false indication, especially in desert areas with large temperature differences between day and night. The foam-based composite phase change material produced by the present invention can be used as an insert in combination with a tent, and light energy is stored in the form of heat energy during the day through photothermal conversion, and the heat energy stored during the day is released at night to achieve a heat preservation effect (see Fig.10 ).
[0010] The first object of the present invention is to provide a method for preparing a foam-based phase change composite material, the method comprising the following steps:
[0011] (1) dispersing molybdenum disulfide in an adhesive precursor solution to form a mixed solution;
[0012] (2) using the foam as a matrix and then immersing it in the mixed solution obtained in step (1) to obtain a foam matrix with surface modified MoS2 nanoparticles;
[0013] (3) After carbonization, the foam matrix of the surface-modified MoS2 nanoparticles in step (2) is added to the molten phase change material and vacuum adsorbed to obtain a foam-based phase change composite material.
[0014] In one embodiment of the present invention, the adhesive in step (1) is polydimethylsiloxane (PDMS).
[0015] In one embodiment of the present invention, the solvent of the adhesive precursor in step (1) is n-hexane.
[0016] In one embodiment of the present invention, the concentration of the adhesive in the adhesive precursor solution in step (1) is 2-4 mg / mL.
[0017] In one embodiment of the present invention, the concentration of molybdenum disulfide in the mixed solution in step (1) is 20-40 mg / mL.
[0018] In one embodiment of the present invention, the mixed solution in step (1) needs to be ultrasonicated in an ultrasonic vibrator for 0.5 to 2 hours.
[0019] In one embodiment of the present invention, the foam matrix in step (2) is melamine foam (MF).
[0020] In one embodiment of the present invention, the soaking time in step (2) is 0.5 to 2 hours.
[0021] In one embodiment of the present invention, ultrasonic vibration is performed while soaking in step (2).
[0022] In one embodiment of the present invention, the carbonization in step (3) is carried out under a N2 atmosphere at 300-600°C for 2-4h.
[0023] In one embodiment of the present invention, the phase change composite material in step (3) includes paraffin, soybean wax, higher aliphatic hydrocarbons and their eutectics, fatty acids and their eutectics, fatty acid esters, alcohols, polyhydroxycarbonates, polyolefins, and polyols.
[0024] In one embodiment of the present invention, the phase change material in step (3) is polyethylene glycol-6000 (PEG-6000).
[0025] The present invention provides a foam-based phase-change composite material prepared as described above.
[0026] The second object of the present invention is to provide a foam-based phase change composite material for a nighttime desert thermal insulation tent using the above method.
[0027] The third object of the present invention is to apply the above foam-based phase change composite material to the field of thermal energy storage and release.
[0028] The fourth object of the present invention is to apply the above foam-based phase change composite material to the field of thermal insulation.
[0029] The fifth object of the present invention is to apply the above-mentioned foam-based phase change composite material to the fields of light-heat conversion, infrared stealth and false indication, or outdoor thermal insulation in areas with large temperature differences between day and night.
[0030] Beneficial effects of the present invention:
[0031] 1. The porous foam matrix required by the present invention is MF, which is easy to cut and has no size restrictions. MF is safe and non-toxic, has a wide source and is inexpensive. Moreover, MF has excellent mechanical properties, is light and flexible, and has a three-dimensional network porous structure inside, which can better encapsulate PCMs and enable it to be combined with the tent without leakage.
[0032] 2. Carbonization improves the ability of the foam skeleton to capture photons, giving the foam skeleton a certain ability to convert light into heat. At the same time, MoS2 nanoparticles have an inherent band gap, a unique layered structure, and a wide range of visible light and near-infrared absorption, which have good light-to-heat conversion capabilities, further improving the light-to-heat conversion capabilities of the foam skeleton, making it possible to convert daytime light energy into heat energy for storage in desert areas with large temperature differences between day and night. Moreover, after the MoS2 nanoparticles are attached to the foam skeleton, the roughness of the foam skeleton is increased, and the adsorption capacity of the foam pores is increased, thereby better encapsulating PCMs.
[0033] 3. The lightweight flexible carbon foam-based phase change composite material provided by the present invention has a controllable heat storage capacity and can store up to 95% of phase change material. Its controllability lies in that the purpose of controlling the heat storage capacity of the composite material can be achieved by controlling the mass percentage of the phase change material adsorbed by vacuum, and it can be applied to fields with different heat capacity requirements. The phase change material is a solid-liquid phase change material, which can be one or more of paraffin, soybean wax, higher aliphatic hydrocarbons and their eutectics, fatty acids and their eutectics, fatty acid esters, alcohols, polyhydroxycarbonic acids, polyolefins, polyols, etc., and has high latent heat of phase change, good thermal stability, and high efficiency of heat energy storage and release. It can be used in the fields of heat energy storage, thermal insulation, solar energy storage, photothermal conversion, infrared stealth and false indication. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 Flow charts were prepared for Examples 1, 2, and 3;
[0035] Figure 2 SEM images of different samples: (a) MF@PEG; (b) CMF@PEG; (c) CMFP@PEG; (d) CMFP-3MoS2@PEG;
[0036] Figure 3 Leakage prevention performance test diagram
[0037] Figure 4 Infrared thermal images of different samples on a heating platform at 80°C;
[0038] Figure 5 The temperature variation curve of different samples on the 80℃ heating stage over time;
[0039] Figure 6 The DSC test results are as follows: Figure a is the melting endothermic curve of the phase change material; Figure b is the crystallization exothermic curve of the phase change material;
[0040] Figure 7 Comparison of DSC curves (a) and enthalpy change (b) after 50 thermal cycles in Example 1;
[0041] Figure 8 To test the photothermal conversion performance;
[0042] Fig. 9 This is a comparison diagram of the CMFP-3MoS2 foam in Example 1 and the foam in Comparative Example 4 before and after 50 presses;
[0043] Fig.10 The temperature regulation principle of foam-based phase change composite materials used in nighttime desert insulation tents. DETAILED DESCRIPTION
[0044] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explaining the present invention and are not used to limit the present invention.
[0045] Example 1
[0046] 100 mL of n-hexane was added to a beaker, and then 0.3 g of polydimethylsiloxane and 3 g of MoS2 nanoparticles were added to the beaker to prepare a dispersion liquid. The beaker containing the dispersion liquid was stirred on a magnetic stirring table for 30 min, and then the beaker was placed in an ultrasonic machine for ultrasonic dispersion for 1 h to obtain a uniformly dispersed MoS2 dispersion liquid.
[0047] After washing the melamine foam (MF) with deionized water and ethanol, the size was cut into 2×2×1cm, and the cut MF was immersed in MoS2 dispersion. The excellent adhesion of PDMS was used to adhere MoS2 nanoparticles to the carbon foam skeleton, and then ultrasonicated in an ultrasonic machine for 1h. After that, the MF with MoS2 nanoparticles adhered to the skeleton was taken out and dried in an oven, and then placed in a tubular furnace in a N2 atmosphere for carbonization for 3h, the carbonization temperature was 400℃, and the heating rate was 5℃ / min, and the sample CMFP-3MoS2 was obtained.
[0048] Adsorption of solid-liquid phase change material polyethylene glycol-6000 (PEG-6000) by vacuum melting method: First, the solid-liquid phase change material PEG-6000 is placed in a high-temperature oven to melt. Secondly, CMFP-3MoS2 is placed in the molten PEG-6000 and vacuumed to allow PEG-6000 to be fully adsorbed into the carbon foam. It is left to stand for 3 hours under vacuum, and then the excess phase change material on the sample surface is taken out and adsorbed with filter paper. Finally, after the sample is cooled to room temperature, the phase change material solidifies to obtain the phase change composite material CMFP-3MoS2@PEG.
[0049] Example 2
[0050] 100 mL of n-hexane was added to a beaker, and then 0.3 g of polydimethylsiloxane and 2 g of MoS2 nanoparticles were added to the beaker to prepare a dispersion liquid. The beaker containing the dispersion liquid was stirred on a magnetic stirring table for 30 min, and then the beaker was placed in an ultrasonic machine for ultrasonic dispersion for 1 h to obtain a uniformly dispersed MoS2 dispersion liquid.
[0051] The remaining steps were carried out with reference to Example 1, and finally the phase change composite material CMFP-2MoS2@PEG was obtained.
[0052] Example 3
[0053] 100 mL of n-hexane was added to a beaker, and then 0.3 g of polydimethylsiloxane and 1 g of MoS2 nanoparticles were added to the beaker to prepare a dispersion liquid. The beaker containing the dispersion liquid was stirred on a magnetic stirring table for 30 min, and then the beaker was placed in an ultrasonic machine for ultrasonic dispersion for 1 h to obtain a uniformly dispersed MoS2 dispersion liquid.
[0054] The remaining steps were carried out with reference to Example 1, and finally the phase change composite material CMFP-1MoS2@PEG was obtained.
[0055] Comparative Example 1
[0056] 100 mL of n-hexane was added to a beaker, and then 0.3 g of polydimethylsiloxane was added to the beaker to prepare a dispersion liquid. The beaker containing the dispersion liquid was stirred on a magnetic stirring table for 30 minutes, and then the beaker was placed in an ultrasonic machine for ultrasonic dispersion for 1 hour to obtain a polydimethylsiloxane dispersion liquid.
[0057] The remaining steps were carried out with reference to Example 1, and finally the phase change composite material CMFP@PEG was obtained.
[0058] Comparative Example 2
[0059] Melamine foam (MF) was washed with deionized water and ethanol successively, and then cut into 2×2×1 cm in size. The foam was taken out and dried in an oven, and then carbonized in a tubular furnace in a N2 atmosphere for 3 h. The carbonization temperature was 400°C and the heating rate was 5°C / min.
[0060] The solid-liquid phase change material polyethylene glycol-6000 (PEG-6000) was adsorbed by the vacuum melting method: first, the solid-liquid phase change material PEG-6000 was melted in a high-temperature oven. Secondly, the carbonized foam matrix was placed in the molten PEG-6000 and vacuumed to allow PEG-6000 to be fully adsorbed into the carbon foam. After vacuuming twice, the sample was allowed to stand in a vacuum state for 3 hours, and then filter paper was used to adsorb the excess phase change material on the surface of the sample material. Finally, after the sample was cooled to room temperature, the phase change material was solidified to obtain the phase change composite material CMF@PEG.
[0061] Comparative Example 3
[0062] Melamine foam (MF) was washed with deionized water and ethanol successively, and then cut into a size of 2×2×1 cm.
[0063] The solid-liquid phase change material polyethylene glycol-6000 (PEG-6000) was adsorbed by the vacuum melting method: first, the solid-liquid phase change material PEG-6000 was melted in a high-temperature oven. Secondly, the carbonized foam matrix was placed in the molten PEG-6000 and vacuumed to allow PEG-6000 to be fully adsorbed into the foam. After vacuuming twice, the sample was allowed to stand for 3 hours under vacuum, and then filter paper was used to adsorb the excess phase change material on the surface of the sample material. Finally, after the sample was cooled to room temperature, the phase change material solidified to obtain the phase change composite material MF@PEG.
[0064] Comparative Example 4
[0065] 100 mL of n-hexane was added to a beaker, and then 0.3 g of polydimethylsiloxane and 3 g of MoS2 nanoparticles were added to the beaker to prepare a dispersion liquid. The beaker containing the dispersion liquid was stirred on a magnetic stirring table for 30 min, and then the beaker was placed in an ultrasonic machine for ultrasonic dispersion for 1 h to obtain a uniformly dispersed MoS2 dispersion liquid (the mass percentage concentration of MoS2 nanoparticles was 3%).
[0066] Melamine foam (MF) was washed with deionized water and ethanol, then taken out and dried in an oven, and then carbonized in a tubular furnace in a N2 atmosphere for 3 hours at a carbonization temperature of 400°C and a heating rate of 5°C / min to obtain CMF. CMF was cut into 2×2×1cm pieces, and the cut CMF was immersed in a MoS2 dispersion, and the mixed solution was reacted in an ultrasonic machine for 1 hour. The sample was taken out and dried to obtain a sample named CMF-P 3MoS2.
[0067] Performance Testing
[0068] The foam-based composite phase change materials prepared in Example 1 and Comparative Examples 1 to 3 were subjected to a packaging anti-leakage test (see Figure 3 ), it can be found that the foam-based composite phase change materials prepared in Example 1 and Comparative Examples 1 to 3 have excellent encapsulation capabilities. After being heated in an oven at 80°C for 50 min, no obvious PEG leakage occurred, while MF@PEG had PEG leakage.
[0069] The foam-based composite phase change materials prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were tested for thermal properties. The samples were placed on a heating table at 80°C and heated for 20 minutes. The temperature changes were recorded using an infrared thermal imager (see Figure 4 ), its temperature variation trend with time (see Figure 5 ) It can be seen that: the sample of Example 1 has the best thermal conductivity and the fastest temperature rise; the samples of Examples 2 to 3 have faster thermal conductivity and faster temperature rise, which are higher than the samples without adding MoS2 nanoparticles, indicating that MoS2 nanoparticles help the foam skeleton to conduct heat.
[0070] The foam-based composite phase change materials prepared in the above Examples 1 to 3 and Comparative Examples 1 to 3 were subjected to DSC (see Figure 6 ) analysis, the sample prepared in Example 1 has a melting temperature of 61.8°C, a melting enthalpy of 159.8 J / g, a crystallization temperature of 39.4°C, and a crystallization enthalpy of 146.6 J / g; the sample prepared in Example 2 has a melting temperature of 62.1°C, a melting enthalpy of 162.0 J / g, a crystallization temperature of 42.3°C, and a crystallization enthalpy of 151.8 J / g; the sample prepared in Example 3 has a melting temperature of 64.7°C, a melting enthalpy of 163.7 J / g, a crystallization temperature of 41.9°C, and a crystallization enthalpy of 154.9 J / g; the melting temperature of the sample prepared in Comparative Example 1 is 60.2°C, the melting enthalpy is 163.4J / g, the crystallization temperature is 37.8°C, and the crystallization enthalpy is 139.6J / g; the melting temperature of the sample prepared in Comparative Example 2 is 60.4°C, the melting enthalpy is 167.1J / g, the crystallization temperature is 39.7°C, and the crystallization enthalpy is 144.0J / g; the melting temperature of the sample prepared in Comparative Example 3 is 60.5°C, the melting enthalpy is 146.7J / g, the crystallization temperature is 36.8°C, and the crystallization enthalpy is 127.5J / g.
[0071] DSC curve of the foam-based composite phase change material after 50 thermal cycles (see Figure 7 a), enthalpy change before and after the cycle (see Figure 7 b), it is not difficult to see that the DSC curve and enthalpy value of the sample in Example 1 change very little before and after 50 thermal cycles, indicating that the sample in Example 1 has excellent stability.
[0072] The results of the light-heat conversion test of the foam-based composite phase change materials prepared in the above Examples 1 to 3 and Comparative Examples 1 to 3 (see Figure 8). After ten minutes of light exposure, the temperature inside the phase change material of Example 1 rises from 20°C to 92°C, and the phase change material changes from solid to liquid; the temperature inside the phase change material of Example 2 rises from 20°C to 87°C, and the phase change material changes from solid to liquid; the temperature inside the phase change material of Example 3 rises from 20°C to 81°C, and the phase change material changes from solid to liquid; the temperature inside the phase change material of Comparative Example 1 rises from 20°C to 76°C, and the phase change material changes from solid to liquid; the temperature inside the phase change material of Comparative Example 2 rises from 20°C to 74°C, and the phase change material changes from solid to liquid; the temperature inside the phase change material of Comparative Example 3 rises from 20°C to 60°C, and the solid phase change material does not change to liquid. It can be seen that the foam-based composite phase change materials of Examples 1 to 3 have excellent light-to-heat conversion capabilities, and from the slope of the curve, it can be seen that the temperature rise rate during this period is higher than that of the sample without nanoparticles, namely, Comparative Example 1, which shows that the MoS2 nanoparticles on the foam skeleton effectively improve the light-to-heat conversion efficiency of the phase change composite material, while the foam-based composite phase change material of Comparative Example 3 does not have light-to-heat conversion capabilities. In addition, the foam-based composite phase change material of Example 1 has the most excellent light-to-heat conversion capability, can realize the storage of light energy, has the ability to collect clean energy such as solar energy, can convert daytime light energy into heat energy for storage in desert areas, and release it in the form of heat energy at night.
[0073] The foam-based composite phase change materials prepared in Example 1 and Comparative Example 4 were subjected to 50 mechanical compression tests. The results are shown in Fig. 9 , it can be seen that the elastic recovery performance of first adhering MoS2 molybdenum disulfide nanoparticles to the MF skeleton with PDMS and then decarbonizing it is better than that of first carbonizing MF into CMF.
[0074] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.
Claims
1. A method for preparing a foam-based phase change composite material for a nighttime desert thermal insulation tent, characterized in that: The method comprises the following steps: (1) dispersing MoS2 in an adhesive precursor solution to form a mixed solution; (2) using the foam as a matrix and then immersing it in the mixed solution obtained in step (1) to obtain a foam matrix with surface modified MoS2 nanoparticles; (3) After carbonization, the foam matrix with MoS2 nanoparticles modified on the surface in step (2) is immersed in a phase change material melt and vacuum adsorbed to obtain a foam-based phase change composite material.
2. The preparation method according to claim 1, characterized in that: The adhesive in step (1) is polydimethylsiloxane.
3. The preparation method according to claim 1, characterized in that: The solvent of the adhesive precursor in step (1) is n-hexane.
4. The preparation method according to claim 1, characterized in that: In step (1), the concentration of the adhesive in the adhesive precursor solution is 2 to 4 mg / mL; the concentration of MoS2 in the mixed solution is 20 to 40 mg / mL.
5. The preparation method according to claim 1, characterized in that: In step (2), the foam matrix is melamine foam.
6. The preparation method according to claim 1, characterized in that: In step (2), the soaking time is 0.5 to 2 hours; ultrasonic vibration is performed while soaking.
7. The preparation method according to claim 1, characterized in that: In step (3), carbonization is carried out under N2 atmosphere at 300-600°C for 2-4h.
8. The preparation method according to claim 1, characterized in that: The phase change composite material in step (3) includes paraffin wax, soybean wax, higher aliphatic hydrocarbons and their eutectics, fatty acids and their eutectics, fatty acid esters, alcohols, polyhydroxycarbonates, polyolefins, and polyols.
9. A foam-based phase change composite material for a nighttime desert thermal insulation tent, characterized in that: The foam-based phase change composite material for the nighttime desert thermal insulation tent is prepared according to the method described in any one of claims 1 to 8.
10. Application of the foam-based phase change composite material for nighttime desert thermal insulation tents as claimed in claim 9 in the fields of light-heat conversion, infrared stealth and false indication, or outdoor thermal insulation in areas with large temperature differences between day and night.