Sna&beta-G (at) Cu / Fe-TADS biological composite material with graded holes and preparation method and application of Sna&beta-G (at) Cu / Fe-TADS biological composite material

By preparing Sna&β-G@Cu/Fe-TADS biocomposite with graded pores, the problems of reduced enzyme activity and mass transfer in enzyme immobilized materials are solved, and efficient preparation of rare ginseng saponin CK and enhancement of enzyme stability are achieved, thereby promoting the promotion of The industrial application of biocomposite materials.

CN118956856APending Publication Date: 2024-11-15XI'AN POLYTECHNIC UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411033016.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing enzyme immobilized materials have reduced enzyme activity in confined spaces, and the mass transfer problem leads to low enzyme load and poor leaching rate. There are toxic media during the preparation process, which affects industrial application.

Method used

Using the organic ligands with good water-soluble disodium terephthalate and ferrous ions, Sna&β-G@Cu/Fe-TADS biocomposite with fractionated pores is prepared through metal competition and oxidation, for cascade catalysis of enzymes. , ensure that the enzyme structure is not destroyed and in-situ encapsulation is achieved.

Benefits of technology

It improves the catalytic conversion efficiency of enzymes, compensates for mass transfer problems, reduces the cost of material preparation, realizes efficient preparation of rare ginseng saponin CK, and improves the stability and reusability of enzymes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956856A_ABST
    Figure CN118956856A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of biological composite materials, and particularly relates to Snaamp with graded holes. The invention discloses a beta-G (at) Cu / Fe-TADS biological composite material and a preparation method and application thereof, and the preparation method comprises the following steps: selecting an organic ligand disodium terephthalate with good water solubility, introducing ferrous ions, and preparing Snaamp containing hierarchical pores through a metal competition strategy; the beta-G (at) Cu / Fe-TADS is used for cascade catalysis of ginsenoside Rb1 to prepare rare ginsenoside CK, graded pore channels can promote mass transfer of a substrate and a product, and large pore channels are beneficial to effective exposure of other pore channels, so that effective contact between enzyme and the substrate is increased, and the catalytic conversion effect of the enzyme is played to the greatest extent. The Snaamp is effectively compensated; in the amplification preparation process of the beta-G coated H-Cu-BDC biological composite material, the problem of hollow cavity disappearance caused by mass transfer is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of biocomposite materials, and in particular relates to a Sna&β-G@Cu / Fe-TADS biocomposite material with graded pores, a preparation method thereof and an application thereof. Background Art

[0002] Rare ginsenoside CK has good medicinal value, such as anti-cancer, anti-inflammatory and anti-fatigue. However, it does not exist in natural products. Enzymatic hydrolysis has become the most popular preparation method due to its mild operating conditions, high specificity and environmental friendliness. Enzymatic hydrolysis has attracted widespread attention due to its high efficiency and specificity. However, enzymes are easily denatured and inactivated in irritating environments (such as strong acids, strong bases and organic solvents) and are difficult to separate from the reaction system after use, resulting in the presence of by-products in the product, resulting in low purity and non-recyclable enzymes, which makes the cost of enzymatic hydrolysis high. Enzyme immobilization has become an effective means to solve the problem of enzyme sensitivity and inactivation, which can greatly improve the stability and reusability of enzymes, reduce the cost of enzyme use and promote continuous production in industrial applications. However, most immobilization materials fix the enzyme in a relatively closed space, which is not conducive to the activity of the enzyme. For example, tightly packed enzymes in the host material usually lack conformational freedom, which may greatly affect molecular recognition. The mass transfer of substrates or products may also become a limiting factor, so the activity of the restricted enzyme will be significantly reduced. In addition, traditional immobilization methods suffer from low enzyme loading and high leaching rates due to weak interactions or pore size mismatch. Therefore, there is an urgent need to explore new immobilization materials to overcome these challenges and achieve optimal enzyme performance in confined spaces.

[0003] In order to solve this kind of problem, the immobilized enzyme technology was created in the 1960s and in-depth research was carried out. Among them, MOF has become an excellent carrier for enzyme immobilization due to its adjustable structure, high porosity and high specific surface area. In order to accelerate the rate-limiting step in the preparation process of rare ginsenosides, multiple enzymes are co-immobilized on the MOF carrier, which can not only effectively exert the cascade catalytic efficiency of the enzyme, but also the good stability of the MOF carrier provides a mild and stable environment for the enzyme, shortens the substrate mass transfer distance, improves the time-space yield, reduces the reactor volume, shortens the cycle time and reduces the unit operation. Therefore, based on the research results obtained, it is of great economic value to explore the transformation and application of MOF carrier immobilized dual enzymes for rare ginsenoside CK.

[0004] In order to further promote the industrial application of enzyme@MOF biocomposites, adhering to the concept of green chemistry, we are committed to removing toxic media in the preparation process of such biocomposites, realizing the preparation of enzyme@MOF biocomposites in aqueous conditions, reducing the preparation cost of materials and achieving the purpose of efficient conversion. The existing technology improves the strategy of preparing hollow MOFs by protein soft template method, co-immobilizes Sna and β-G, and prepares Sna&β-G@H-Cu-BDC biocomposites. During the scale-up preparation process of this biocomposite, the hollow cavity disappears due to mass transfer problems, affecting the catalytic conversion of the enzyme. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a Sna&β-G@Cu / Fe-TADS bio-composite material with hierarchical pores, and a preparation method and application thereof. The present invention selects disodium terephthalate, an organic ligand with good water solubility, and introduces ferrous ions to prepare Sna&β-G@Cu / Fe-TADS with hierarchical pores through metal competition and oxidation, which is used for cascade catalysis of ginsenoside Rb1 to prepare rare ginsenoside CK.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] A method for preparing a Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores comprises the following steps:

[0008] Under stirring conditions, snail enzyme and β-glycosidase were mixed with sodium deoxycholate solution, and then Cu 2+ Aqueous solution and Fe 2+ aqueous solution, encapsulating snail enzyme and β-glycosidase in Cu / Fe-NaDC hydrogel, keeping the enzyme protein structure intact, and generating Sna&β-G@Cu / Fe-NaDC hydrogel;

[0009] Under stirring conditions, an organic ligand disodium terephthalate is added to the Sna&β-G@Cu / Fe-NaDC hydrogel, and the organic ligand captures the metal ions in the hydrogel, and a Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores is prepared through oxidation and metal competitive coordination.

[0010] In a preferred embodiment of the present invention, it is characterized in that NaDC, Cu 2+ , the molar ratio of disodium terephthalate is 1:2:0.5~1.

[0011] In a preferred embodiment of the present invention, Cu 2+ with Fe 2+ The molar ratio is 1:1.

[0012] In a preferred embodiment of the present invention, the total synthesis time of the biocomposite material is 3.5 h, the magnetic stirring time when preparing the hydrogel is 0.5 h, and the magnetic stirring time when preparing the composite material is 3 h.

[0013] In a preferred embodiment of the present invention, the ratio of the amount of snail enzyme and β-glycosidase added to the amount of sodium deoxycholate solution is 50 mg:5 mL, wherein the concentration of sodium deoxycholate solution is 29 mg / mL

[0014] In a preferred embodiment of the present invention, the mass ratio of helicase to β-glycosidase is 49.752:0.248.

[0015] In a preferred embodiment of the present invention, the Cu 2+ The aqueous solution is copper acetate solution, Fe 2+ The solution is ferrous acetate solution.

[0016] In a preferred embodiment of the present invention, the molar ratio of the ferrous acetate solution to disodium terephthalate is 1:2.

[0017] Another object of the present invention is to provide a Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores obtained by any of the preparation methods described above.

[0018] The third object of the present invention is to provide an application of the Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores as described in claim 8 in the catalytic conversion of ginsenosides, characterized in that the Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores is used to catalytically convert ginsenoside Rb1 to prepare ginsenoside CK.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The present invention encapsulates snail enzyme and β-glycosidase in Cu 2+ / Fe 2+ -NaDC hydrogel, the good biocompatibility of the hydrogel can protect the enzyme from the stimulation of metal ions and organic ligands, ensure that the structure of the protein is not destroyed, and maximize the catalytic conversion of the enzyme. Then, the organic ligand disodium terephthalate is added. The organic ligand captures the metal ions in the hydrogel, and the hydrogel gradually breaks directly to form a flower-like MOF composed of a layered structure, realizing the in-situ encapsulation of the enzyme on the MOF carrier. At the same time, during the material synthesis process, the added Fe 2+ With Cu 2+ Competitive coordination is formed, Fe 2+ Due to the preferential coordination with the carboxyl group, the organic ligand is first combined with the coordination bond, and then due to oxidation, Fe2+ Oxidized to Fe 3+ The bonding interaction with the coordination bonds was weakened, resulting in the breaking of some coordination bonds to form coordination defects. Finally, a flower-like Sna&β-G@Cu / Fe-TADS biocomposite material containing hierarchical channels was prepared through oxidation and metal competitive coordination.

[0021] 2. The present invention selects disodium terephthalate, an organic ligand with good water solubility, and introduces ferrous ions. The Sna&β-G@Cu / Fe-TADS containing hierarchical pores is prepared through a metal competition strategy for cascade catalysis of ginsenoside Rb1 to prepare rare ginsenoside CK. The hierarchical pores can not only promote the mass transfer of substrate and product, but also the large pores are conducive to the effective exposure of other pores, thereby increasing the effective contact between the enzyme and the substrate, maximizing the catalytic conversion effect of the enzyme, and effectively compensating for the disappearance of the hollow cavity caused by mass transfer problems during the scale-up preparation of the Sna&β-G@H-Cu-BDC biocomposite material.

[0022] 3. The present invention uses Sna&β-G@H-Cu-BDC as a model to achieve the goal of preparing enzyme@MOF biocomposite materials under aqueous conditions by exchanging the organic ligand terephthalic acid corresponding to the water-soluble sodium salt disodium terephthalate. Secondly, Fe 2+ Through its oxidation and Cu 2+ The Sna&β-G@Cu / Fe-TADS biocomposite containing hierarchical channels was prepared by the competitive coordination effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a research idea diagram for the present invention;

[0024] Figure 2 Schematic diagram of the synthesis process of Sna&β-G@Cu / Fe-TADS biocomposite under aqueous conditions of bimetallic competitive coordination;

[0025] Figure 3 Effects of TADS dosage (a), metal ion ratio (b), enzyme dosage (c) and synthesis time (d) on the relative enzyme activity and loading of Sna&β-G@Cu / Fe-TADS biocomposites;

[0026] Figure 4 SEM images of Sna&β-G@Cu / Fe-TADS biocomposite materials at different synthesis times: (a) 30min+30min; (b) 30min+60min; (c) 30min+90min; (d) 30min+120min; (e) 30min+150min; (f) 30min+180min;

[0027] Figure 5 SEM images and EDS images of Cu / Fe-TADS (a) and Sna&β-G@Cu / Fe-TADS biocomposite (b);

[0028] Figure 6 Bright field (a) and fluorescence field (b) of confocal laser microscopy imaging of Sna&β-G@Cu / Fe-TADS biocomposite, dual-channel mode of CLSM, (c) and (d), single-channel mode of CLSM;

[0029] Figure 7 N2 adsorption isotherms (a), pore size distribution (b) and particle size distribution curves (c) of Sna&β-G@H-Cu-BDC, Sna&β-G@Cu / Fe-TADS(20) and Sna&β-G@Cu / Fe-TADS(200);

[0030] Figure 8 TGA curves of Cu / Fe-TADS, Sna&β-G@Cu / Fe-TADS(20) and Sna&β-G@Cu / Fe-TADS(200);

[0031] Fig. 9 XRD spectra of Cu-BDC, Cu / Fe-TADS, Sna&β-G@Cu / Fe-TADS(20) and Sna&β-G@Cu / Fe-TADS(200);

[0032] Fig.10 FTIR spectra of Cu / Fe-TADS, Sna&β-G@Cu / Fe-TADS(20) and Sna&β-G@Cu / Fe-TADS(200);

[0033] Fig.11 XPS spectra of Cu / Fe-TADS, Sna&β-G@Cu / Fe-TADS(20) and Sna&β-G@Cu / Fe-TADS(200) (a), extended scan spectra in the Fe 2p (b), Cu 2p (c), C 1s (d), O1s (e) and N 1s (f) regions;

[0034] Fig.12 pH stability (a), temperature stability (b), organic solvent tolerance (c), and storage stability (d) of free Sna and β-G and Sna&β-G@Cu / Fe-TADS (20);

[0035] Fig.13 The effect of the scale-up preparation system of Sna&β-G@Cu / Fe-TADS biocomposite on relative enzyme activity and enzyme loading;

[0036] Fig.14 SEM images of the scaled-up preparation system of Sna&β-G@Cu / Fe-TADS biocomposite materials, (a) Control; (b) 40mL; (c) 60mL; (d) 80mL; (e) 100mL; (f) 200mL;

[0037] Fig.15 SEM images of Cu / Fe-TADS loaded with and without enzyme in 20 mL and 200 mL systems: (a) normal system with enzyme; (b) normal system without enzyme; (c) enlarged system with enzyme; (d) enlarged system without enzyme.

[0038] Fig.16 is the CK conversion rate and concentration of Sna&β-G@Cu / Fe-TADS biocomposite at different conversion times;

[0039] Fig.17 is the relative enzyme activity of Sna&β-G@Cu / Fe-TADS biocomposite after 6 cycles;

[0040] Fig.18 The CK conversion rate and concentration of the Sna&β-G@Cu / Fe-TADS biocomposite scale-up conversion system;

[0041] Fig.19 The sedimentation performance of Sna&β-G@Cu / Fe-TADS biocomposite materials, (a) 0min; (b) 30min; (c) 60min; (d) 120min; (e) 180min; (f) 240min;

[0042] Fig. 20 The effect of different sedimentation times on the relative enzyme activity and loading of Sna&β-G@Cu / Fe-TADS biocomposites;

[0043] Fig.21 SEM images of Sna&β-G@Cu / Fe-TADS biocomposites at different sedimentation times: (a) Control; (b) 3h; (c) 6h; (d) 12h; (e) 24h. DETAILED DESCRIPTION

[0044] The following is a detailed description of the technical solutions in the embodiments of the present invention in combination with the preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] It should be noted that all professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.

[0046] Example 1

[0047] A method for preparing a Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores comprises the following steps:

[0048] (1) 50 mg of snail enzyme (Sna) and β-glycosidase (β-G) were quickly mixed with 5 mL (29 mg / mL) of sodium deoxycholate (NaDC) solution, and then 5 mL (13.96 mg / mL) of copper acetate solution and 5 mL (13.36 mg / mL) of ferrous acetate solution were added and magnetically stirred for 30 min to generate Sna@β-G@Cu / Fe-NaDC hydrogel;

[0049] (2) Add 5 mL (7.92 mg / mL) of disodium terephthalate solution to the Sna@β-G@Cu / Fe-NaDC hydrogel prepared in step (1), and stir magnetically for 3 h to obtain the Sna&β-G@Cu / Fe-TADS biocomposite material. Finally, the material is collected by the same collection method as that of the prior art for preparing the Sna&β-G@Cu-BDC biocomposite material.

[0050] Example 2

[0051] The difference from Example 1 is that sodium deoxycholate, Cu 2+ , and disodium terephthalate are in a molar ratio of 1:2:1.

[0052] Comparative Example 1

[0053] The difference from Example 1 is that sodium deoxycholate, Cu 2+ , and the molar ratio of disodium terephthalate is 1:2:1.5.

[0054] Comparative Example 2

[0055] The difference from Example 1 is that sodium deoxycholate, Cu 2+ , and disodium terephthalate are in a molar ratio of 1:2:2.

[0056] Comparative Example 3

[0057] The difference from Example 1 is that sodium deoxycholate, Cu 2+ , and the molar ratio of disodium terephthalate is 1:2:2.5.

[0058] Comparative Example 4

[0059] The difference from Example 1 is that sodium deoxycholate, Cu 2+ , and disodium terephthalate are in a molar ratio of 1:2:3.

[0060] Comparative Example 5

[0061] The difference from Example 1 is that Cu 2+ with Fe 2+ The molar ratio is 1:2.

[0062] Comparative Example 6

[0063] The difference from Example 1 is that Cu 2+ with Fe 2+ The molar ratio is 1:3.

[0064] Comparative Example 7

[0065] The difference from Example 1 is that Cu 2+ with Fe 2+ The molar ratio is 2:1.

[0066] Comparative Example 8

[0067] The difference from Example 1 is that Cu 2+ with Fe 2+ The molar ratio is 2:3.

[0068] Comparative Example 9

[0069] The difference from Example 1 is that Cu 2+ with Fe 2+ The molar ratio is 3:1.

[0070] Comparative Example 10

[0071] The difference from Example 1 is that the magnetic stirring time is 30min+30min.

[0072] Comparative Example 11

[0073] The difference from Example 1 is that the magnetic stirring time is 30min+60min.

[0074] Comparative Example 12

[0075] The difference from Example 1 is that the magnetic stirring time is 30min+90min.

[0076] Comparative Example 13

[0077] The difference from Example 1 is that the magnetic stirring time is 30min+120min.

[0078] Comparative Example 14

[0079] The difference from Example 1 is that the magnetic stirring time is 30min+150min.

[0080] 1. Experimental reagents and instruments

[0081] The experimental reagents and instruments are shown in Tables 1 and 2.

[0082] Table 1 Main chemical reagents

[0083]

[0084]

[0085] Table 2 Experimental instruments

[0086] Instrument Name Manufacturer Electric blast drying oven Tianjin Test Instrument Co., Ltd. Analytical Balance Sartorius Magnetic stirrer IKA Instrument Name Manufacturer UV-Vis Spectrophotometer Shanghai Yuanxi Instrument Co., Ltd. High-speed refrigerated centrifuge Eppendorf, Germany Freeze Dryer Shanghai Zhixin Experimental Instrument Technology Co., Ltd. High performance liquid chromatography Shanghai Daojin Instrument Technology Co., Ltd.

[0087] 2. Characterization methods

[0088] The surface morphology and element distribution of the samples were analyzed using Hitachi Flex SEM 1000 scanning electron microscope (SEM) and energy dispersive spectrometer (EDS). The distribution of enzymes in the Sna&β-G@Cu / Fe-TADS biocomposite was analyzed using a confocal laser scanning microscope (CLSM LSM700). Thermogravimetric analysis (TGA) (METTLER 851e) was performed under N2 atmosphere (10℃ / min). The temperature was increased from room temperature to 800℃. Cu-Ka Radiation, X-ray diffraction (XRD, Rigaku MiniFlex600) was performed at room temperature to study the crystal structure of the sample. A Fourier transform infrared spectrometer (ThermoScientific NicoletiS10) was used to study different functional groups in the range of 400-4000cm-1. The element type and existence form in the sample were determined by X-ray photoelectron spectrometer (XPS, thermoescalab 250XI). After the sample was degassed at 120°C overnight, the N2 adsorption isotherm was measured at a relative pressure of 1.0 using a Quantachrome iQ2 porosimeter to determine the total pore volume. The Brunauer-Emmett-Teller (BET) method and density functional theory (DFT) were used to calculate the specific surface area and study the pore size distribution, respectively.

[0089] 3. Enzyme activity detection and calculation

[0090] The enzyme activity was detected by p-NPG colorimetry. First, 100 μL of p-NPG (1 mmol / mL) and 700 μL of acetic acid buffer (pH = 4.5) were heated in a 50°C water bath for 15 min. Then 100 μL of enzyme solution was added, reacted at 50°C for 5 min, and then 1 ml of Na2CO3 (1 mol / L) was added to terminate the reaction. The solution was placed at room temperature for 5 min and dropped onto a 96-well plate. The absorbance was measured at 405 nm using an enzyme reader. Three parallel experiments were performed for each reaction. Enzyme activity is defined as the amount of enzyme (mg) required to hydrolyze 1 mmol p-NPG per unit time. The enzyme activity calculation formula is as shown in formula (1):

[0091]

[0092] Wherein, Y is the absorbance value at 405 nm; k is the slope of the p-NP standard curve; V1 (mL) is the total volume of the reaction system; b is the longitudinal intercept of the p-NP standard curve; V2 (mL) is the volume of the added enzyme; t (min) is the reaction time of the system.

[0093] 4. Enzyme loading determination

[0094] Take a certain volume (V) of the synthetic reaction supernatant, use the Bradford method, and measure the absorbance at 595nm with UV-2600. Substitute the absorbance into the BSA standard curve to calculate the protein concentration of the supernatant (C1). The mass of the initial added enzyme is recorded as m, and the total mass of the biocomposite material is recorded as M. Calculate the embedding rate and embedding amount of the sample according to formula (2) and formula (3):

[0095]

[0096] Relative embedding amount (mg / g) = (m-C1*V) / M (3)

[0097] 5. Enzyme-catalyzed reaction kinetics analysis

[0098] 0.1 mg of free enzyme and immobilized enzyme were reacted with different concentrations (0.0625-0.5 mmol) of p-NPG. The absorbance at 405 nm was then measured and converted into concentration. The Km and Vm values ​​of free enzyme and immobilized enzyme were calculated using the Linewever-Burk formula.

[0099] 6. Immobilized enzyme conversion of ginsenoside Rb1

[0100] Sna and β-G were immobilized on H-Cu-BDC to obtain Sna@H-Cu-BDC and β-G@H-Cu-BDC, respectively, and the mixture of the two was called mixed immobilization (MI). The mixture of Sna and β-G was immobilized together, which was named co-immobilization (CI).

[0101] Ginsenoside Rb1 (2 mg) was added to an acetate buffer (1 mL) at pH = 4.5, and the enzyme (1 mg) was immobilized. The rare ginsenoside CK was converted at 50 ° C (48 h), and then 800 uL of n-butanol was added to the reaction system for extraction. After mixing and centrifugation, 600 uL of the supernatant organic phase was taken and freeze-dried to obtain the product. The pH, temperature, rotation speed and time of the immobilized enzyme conversion of ginsenoside Rb1 were optimized to improve its conversion rate. In short, 2 mg of Rb1 was reacted with β-G@Cu / Fe-TADS, Sna@Cu / Fe-TADS and Sna&β-G@Cu / Fe-TADS with the same enzyme equivalent at pH = 4.5, 50 ° C, and 100 rpm. After different reaction times, the types and concentrations of the products were determined, and the conversion efficiencies of Sna@Cu / Fe-TADS and β-G@Cu / Fe-TADS, MI and CI on ginsenoside Rb1 were compared, and the effects of single enzyme conversion and double enzyme cascade conversion were evaluated. The effects of different recovery methods (and expanded preparation systems (20, 40, 60, 80, 100 mL) on the Sna&β-G@Cu / Fe-TADS biocomposites were compared. Finally, the effects of different conversion systems on the product conversion efficiency were studied.

[0102] 7. Analysis of transformation products

[0103] The free enzyme and immobilized enzyme containing equal amounts of effective enzyme were reacted with substrate Rb1 at 50°C in acetate buffer solution (pH = 4.5). A certain amount of supernatant was taken every 12 hours and 800 μL of n-butanol was added to vortex extract the unreacted ginsenoside Rb1 and the product ginsenosides Rd, F2, and CK. Then 600 μL of the extract was centrifuged and freeze-dried to obtain the product. The product was dissolved in 400 μL of methanol aqueous solution (methanol: water = 1: 1) and analyzed by high performance liquid chromatography (HPLC, Shimadzu LC-FRBC059). An Agilent ZORBAX Eclipse Plus C18 column (4.6×250mm, 5μm) was used, with a column temperature of 30°C, an injection volume of 20 μL, a wavelength of 210nm, and a flow rate of 0.9mL / min for gradient elution. Solution A was acetonitrile and solution B was aqueous solution. The conditions are shown in Table 3.

[0104] Table 3 HPLC elution conditions

[0105] Time (min) Acetonitrile (%) water(%) 0 35 65 27 35 65 Time (min) Acetonitrile (%) water(%) 37.5 65 35 50.1 65 35

[0106] Three parallel experiments were set up for all experiments, and the mean and standard deviation were calculated. The data were analyzed by variance analysis using Microsoft Excel and Origin 2022.

[0107] Results Analysis

[0108] 1. Synthesis process

[0109] H-Cu-BDC was prepared as a MOF framework by a one-pot method using hydrogel as a soft template. 2+ The organic ligands were replaced with their corresponding water-soluble sodium salt ligands (disodium terephthalate), and a MOF carrier (Cu / Fe-TADS) containing hierarchical channels was successfully prepared under aqueous conditions through oxidation and metal competitive coordination. 2+ / Fe 2+ -NaDC hydrogel, the good biocompatibility of the hydrogel can protect the enzyme from the stimulation of metal ions and organic ligands, keep the protein structure intact, and maximize the catalytic conversion of the enzyme. Then, the organic ligand TADS solution is added, the organic ligand captures the metal ions in the hydrogel, and the hydrogel gradually breaks directly to form a flower-like MOF composed of layered structures, realizing the in-situ encapsulation of the enzyme in the MOF carrier. At the same time, during the material synthesis process, the added Fe 2+ With Cu 2+ Competitive coordination is formed, Fe 2+ Due to the preferential coordination with the carboxyl group, it first combines with the coordination bond of the organic ligand, and then due to oxidation, Fe 2+ Oxidized to Fe 3+ The bonding interaction with the coordination bond is weakened, resulting in the breakage of some coordination bonds to form coordination defects. Finally, the flower-like Sna&β-G@Cu / Fe-TADS biocomposite with hierarchical channels was prepared through oxidation and metal competitive coordination. The specific preparation process is as follows Figure 2 shown.

[0110] 2. Effect of different preparation conditions on the performance of Sna&β-G@Cu / Fe-TADS

[0111] (1) Amount of TADS added

[0112] Firstly, the organic ligand TADS and the metal center Cu 2+ The best ratio. Figure 3 As shown in (a), the addition amount of TADS has a significant effect on the relative enzyme activity and enzyme loading of the Sna&β-G@Cu-TADS biocomposite. 2+When :TADS=1:2:0.5, the relative enzyme activity of Sna&β-G@Cu-TADS biocomposite material is the largest and the enzyme loading reaches 143.25 mg / g. As the amount of TADS added increases, the enzyme loading gradually decreases. The reason may be that at this ratio, the effective collision between metal ions and organic ligands is reduced, resulting in the inability to effectively synthesize the MOF carrier, thereby reducing the enzyme loading. At the same time, the relative enzyme activity of Sna&β-G@Cu-TADS biocomposite material shows a downward trend. The reason may be that the amount of organic ligand added is too high, resulting in the pores of the MOF carrier being blocked, reducing the mass transfer between the substrate and the product.

[0113] (2)Cu 2+ with Fe 2+ The proportion

[0114] The present invention is devoted to 2+ With Cu 2+ The metal competition coordination effect and Fe 2+ The Sna&β-G@Cu / Fe-TADS biocomposite with hierarchical pores was prepared by oxidation. 2+ It can effectively bind to organic ligands. As the reaction proceeds, Fe 2+ Oxidized to Fe 3+ The coordination effect with the organic ligand is weakened, resulting in the breaking of the coordination bond and the generation of coordination defects, which promotes the formation of hierarchical channels in the MOF carrier. Figure 3 From (b), we can see that when Cu 2+ :Fe 2+ =1:1, the relative enzyme activity of Sna&β-G@Cu / Fe-TADS biocomposite was the highest, and the loading amount reached 148.45 mg / g. The reason may be that under this ratio, Fe 2+ The hierarchical pore structure caused by the coordination defects formed by oxidation is more conducive to the transport of substances. At the same time, the large pores are conducive to the exposure of the enzyme active sites, promoting the effective contact between the enzyme and the substrate, thereby increasing the relative enzyme activity of the Sna&β-G@Cu / Fe-TADS biocomposite material.

[0115] (3) Addition amount of Sna and β-G

[0116] The effect of enzyme dosage on the relative enzyme activity and loading capacity of Sna&β-G@Cu / Fe-TADS biocomposites was investigated. Figure 3As shown in (c), when the enzyme dosage is less than 50 mg, the relative enzyme activity and loading of the Sna&β-G@Cu / Fe-TADS biocomposite material show an upward trend with the increase of the dosage. When the enzyme dosage is 50 mg, the relative enzyme activity of the Sna&β-G@Cu / Fe-TADS biocomposite material is the highest, and the loading capacity reaches 152.35 mg / g. However, when the dosage is 60 mg, the relative enzyme activity of the Sna&β-G@Cu / Fe-TADS biocomposite material decreases by 8.25%. The reason may be that the enzyme loading exceeds the saturation loading of the MOF carrier, resulting in ineffective accumulation of the enzyme in the pores, causing blockage of the active center of the enzyme, reducing the effective contact between the enzyme and the substrate, and thus reducing the relative enzyme activity of the Sna&β-G@Cu / Fe-TADS biocomposite material.

[0117] (4) Synthesis time of Sna&β-G@Cu / Fe-TADS

[0118] like Figure 3 As shown in (d), when the synthesis time is 3.5h, the relative enzyme activity of Sna&β-G@Cu / Fe-TADS biocomposite is the highest, and the loading amount reaches 153.25mg / g. As the preparation time increases, the loading amount of Sna&β-G@Cu / Fe-TADS biocomposite remains basically unchanged, but the relative enzyme activity shows a downward trend. The reason may be that the long-term magnetic stirring has an adverse effect on the active center of the enzyme. Therefore, considering the problem of preparation time cost, the optimal preparation time of Sna&β-G@Cu / Fe-TADS biocomposite is finally determined to be 3.5h.

[0119] 3. Analysis of the growth process of Sna&β-G@Cu / Fe-TADS

[0120] In order to explore the growth process of Sna&β-G@Cu / Fe-TADS biocomposites, Figure 4 As shown in (a) to (f), the material morphology at different synthesis times was observed through SEM images. It can be seen from the figure that with the extension of the synthesis time, the Sna&β-G@Cu / Fe-TADS biocomposite material gradually aggregates from the sheet structure. At 3.5h, it presents a flower-like structure. The MOF carrier assembled into a sheet structure not only provides more loading sites for the enzyme, but also the thinner sheet is conducive to the exposure of the enzyme active site, increasing the effective contact between the enzyme and the substrate, and promoting the transfer of the substrate and the product. It effectively solves the problem of material transfer obstruction caused by enzyme immobilization and ensures the efficient catalytic effect of the Sna&β-G@Cu / Fe-TADS biocomposite material.

[0121] 4. Morphology observation

[0122] By comparing the SEM images and EDS images of Cu / Fe-TADS loaded with Sna and β-G ( Figure 5 As shown in (a) and (b), the Cu / Fe-TADS carrier with added enzyme has a smaller particle size than the Sna&β-G@Cu / Fe-TADS biocomposite and does not form a flower-like structure. The reason may be that Fe 2+ The interaction with the amino or carboxyl groups exposed by the protein promotes the formation of the MOF carrier around the enzyme. However, the EDS image shows that in addition to the original C, Cu, and O elements, the appearance of the Fe element can prove the successful coordination of Fe with the organic ligand. In addition, the N element was detected on the surface of the Sna&β-G@Cu / Fe-TADS biocomposite material with the addition of Sna and β-G. It is speculated that the N element comes from the -NH2 of Sna and β-G. The uniform distribution of various elements on the surface of the material further proves the successful synthesis of the material and the successful loading of the enzyme.

[0123] 5. Analysis of enzyme immobilization position

[0124] FITC and RhB were used to label β-G and Sna, respectively, to investigate the successful immobilization of Sna and β-G in Cu / Fe-TADS. Figure 6 (a) to (d)). The labeled β-G and Sna showed red fluorescence at λ = 555-580 and 494-518, respectively. Figure 6 middle (c)) and green fluorescence ( Figure 6 (d)). It can be seen from the figure that Sna and β-G are successfully fixed and evenly distributed in Cu / Fe-TADS, which is consistent with the mapping of N elements in the EDS image. Figure 1 The results further prove that Cu / Fe-TADS is a good carrier of Sna and β-G.

[0125] 6. N2 adsorption curve, pore size and particle size analysis

[0126] Depend on Figure 7As shown in (a), the N2 adsorption isotherms of Sna&β-G@H-Cu-BDC, Sna&β-G@Cu / Fe-TADS(20) and Sna&β-G@Cu / Fe-TADS(200) biocomposites all show type IV isotherm adsorption. The samples show higher N2 absorption at lower relative pressures. As can be seen from the figure, the Sna&β-G@Cu / Fe-TADS(20) biocomposite shows a more obvious desorption hysteresis curve in the pressure range of 0.75-1. The reason may be that the flower-like MOF prepared by metal competitive coordination and oxidation contains a richer pore structure. At the same time, the Sna&β-G@Cu / Fe-TADS(200) biocomposite obtained under a 10-fold magnification of the preparation system also maintains good hierarchical pores, further proving that the scaled-up preparation of the biocomposite within this range is feasible. In addition, by comparing the pore sizes of the three biocomposites ( Figure 7 In (b), it was found that the proportion of pores in the range of 30 nm in the flower-shaped enzyme@MOF biocomposite prepared by metal competitive coordination and oxidation increased significantly, and large pores in the range of 120 nm appeared. The hierarchical pores inside the Sna&β-G@Cu / Fe-TADS biocomposite can not only effectively improve the material transmission efficiency. At the same time, the large pores can promote the exposure of other pores to promote the contact between the substrate and the active species, thereby improving its biocatalytic efficiency. Finally, the particle size of the three biocomposites was compared ( Figure 7 In (c), the results show that due to Fe 2+ The interaction with the amino or carboxyl groups in the protein promotes the growth of MOF around the enzyme, which greatly increases the particle size of the biocomposite. The larger particle size is conducive to the recycling and reuse of the biocomposite. It can effectively reduce its application cost and further promote its industrial application.

[0127] 7. Comparative analysis of stability

[0128] The thermal stability of Cu / Fe-TADS, Sna&β-G@Cu / Fe-TADS(20) and Sna&β-G@Cu / Fe-TADS(200) was tested by TGA. Figure 8As shown, all three materials experienced mass loss in three different stages. First, due to the evaporation of surface adsorbed water and bound water, the weight loss was 8.25% at 25℃-200℃. In addition, when the temperature was greater than 300℃, the material experienced a mass loss of about 42% probably due to the collapse of the MOF skeleton. Among them, the residual mass of the Sna&β-G@Cu / Fe-TADS(20) and Sna&β-G@Cu / Fe-TADS(200) biocomposites was lower than that of the Cu / Fe-TADS carrier without enzyme immobilized. The reason may be caused by the thermal decomposition of the enzyme molecules. The weight loss was consistent with the encapsulation rate, which further proved the successful immobilization of the enzyme. The TGA curve results showed that the prepared MOF carrier had good thermal stability.

[0129] 8. Crystal structure analysis

[0130] Fig. 9 The XRD spectra of Cu-BDC, Cu / Fe-TADS, Sna&β-G@Cu / Fe-TADS(20) and Sna&β-G@Cu / Fe-TADS(200) biocomposites are shown in Figure 2. By comparing and analyzing their crystal structures, it was found that the XRD spectra of the prepared MOF carrier immobilized enzyme and the enlarged preparation system were very consistent with the diffraction pattern of Cu(BDC)(DMF), and Bragg diffraction was detected, indicating that Fe in this ratio range 2+ The addition of did not change the bulk crystal structure of Cu-BDC. The characteristic peaks appeared at 8.22°, 17.3° and 34.5°, corresponding to the 110, 201 and 402 planes of Cu-BDC. Due to the encapsulation of the enzyme, the crystallinity of MOF decreased, resulting in a decrease in the intensity of the diffraction peak. However, the position of the peak did not change, and no new peaks appeared, indicating that the encapsulation of the enzyme did not change the crystal structure of the material. The biocomposite material obtained by this amplified preparation system has good crystal structure characteristics, which further proves that the amplified preparation within this range is effective.

[0131] 9. Analysis of coordination mode

[0132] The FTIR spectra of Cu / Fe-TADS, Sna&β-G@Cu / Fe-TADS(20) and Sna&β-G@Cu / Fe-TADS(200) are shown in Fig.10 The vibrations of the benzene ring correspond to 1509, 1287, 1018, 882, 734 and 567 cm -1 The infrared peaks at 1574 and 1393 cm-1 correspond to the asymmetric and symmetric stretching modes of -COO, respectively. The stretching vibration of Fe-O corresponds to 542 cm -1 , and 569cm -1The characteristic peak at 1655cm belongs to the stretching vibration mode of Cu-O. -1 The signal at 1430 cm corresponds to the stretching vibration of the CO(-CONH) bond in Sna and β-G. -1 The signal at belongs to NH bending and CN stretching vibration, both of which are characteristic peaks of enzymes. This result also proves that the enzyme is successfully embedded in Cu / Fe-TADS. The biocomposite Sna&β-G@Cu / Fe-TADS (200) obtained in the system magnified 10 times also has the same FTIR spectrum, proving that the biocomposite can be successfully prepared within this range. It further provides a basis for its expansion of production.

[0133] 10. Analysis of element existence form

[0134] The elemental compositions and dominant forms of each element in Cu / Fe-TADS, Sna&β-G@Cu / Fe-TADS(20) and Sna&β-G@Cu / Fe-TADS(200) were determined by XPS analysis. The complete spectra of the three samples ( Fig.11 (a) shows that they all contain Cu, Fe, C and O elements, indicating the successful coordination of metal ions with organic ligands. The Fe 2p peaks are located near 711.81eV (2p3 / 2) and 724.81eV (2p1 / 2) ( Fig.11 (b)) belongs to octahedral coordination of Fe 3+ . Cu 2p spectrum ( Fig.11 There are three spin-orbit doublets in (c), Cu 2p 1 / 2 (952.31, 954.52 and 958.23 eV), Cu 2p 3 / 2 (932.14, 935.32 and 938.25 eV) and two satellite peaks (962.41 and 943.53 eV). C 1s has three obvious peaks at 284.80, 286.27 and 288.71 eV ( Fig.11 (d)), corresponding to C=C / CC, CO / CN and C=O, respectively. The peaks of O 1s spectrum at 531.98 eV and 533.25 eV ( Fig.11 (e) corresponds to the coordinated lattice oxygen and crystal water, respectively. The N1s peak at 400.01eV appears in Sna&β-G@H-Cu-BDC ( Fig.11 In (f), the amino acid-derived -NH2 of Sna and β-G is consistent with the results of FTIR spectroscopy, further demonstrating the successful immobilization of the enzyme.

[0135] 11. Comparative analysis of stability

[0136] Generally, when free enzymes are exposed to harsh environments (such as strong acid, strong alkali, high temperature or organic solvents), the conformation of the enzyme will change, resulting in the loss of enzyme activity. Therefore, in order to highlight the good physical protection of Cu / Fe-TADS on enzymes, the relative activities of free enzymes and immobilized enzymes in strong acid, strong alkali, high temperature and organic solvents were compared to further highlight the advantages of MOF-immobilized enzymes.

[0137] (1) pH stability

[0138] The relative enzyme activities of free Sna and β-G and Sna&β-G@Cu / Fe-TADS(20) were compared under different pH conditions (2, 3, 4, 5, 6, 7 and 10). Fig.12 (a)). The results show that the activity of the free enzyme changes significantly after incubation for 6.5 hours in different pH ranges. In particular, after incubation for 6.5 hours under pH = 2 and 10, the enzyme activity is only 26.9% and 9.8% of the initial enzyme activity. The results show that strong acid and alkaline conditions have a greater influence on the activity of the enzyme. It is worth noting that under the same conditions, the enzyme activity of the Sna&β-G@Cu / Fe-TADS(20) biocomposite material is 79.8% and 58.5% of the initial enzyme activity, respectively. The above results prove that compared with the free enzyme, the Sna&β-G@Cu / Fe-TADS(20) biocomposite material broadens the pH application range of the enzyme and increases its tolerance to strong acids and alkalis.

[0139] (2) Temperature stability

[0140] In order to investigate the temperature stability of immobilized enzymes and free enzymes, free Sna and β-G and Sna&β-G@Cu / Fe-TADS(20) biocomposites were incubated at different temperatures (30℃, 40℃, 50℃, 60℃, 70℃, 80℃ and 90℃) for 2.5h. Fig.12 As shown in (b), with the increase of temperature, the relative enzyme activities of both showed a downward trend. In particular, when the temperature was higher than 60°C, the relative activity of the free enzyme decreased significantly, retaining only about 10% of the original enzyme activity. By comparison, it was found that after incubation for 6.5 hours, the relative enzyme activity of the Sna&β-G@Cu / Fe-TADS(20) biocomposite retained about 40% of the initial enzyme activity. The reason may be that Cu / Fe-TADS can effectively protect the conformation of the enzyme from being destroyed, reducing the loss of enzyme activity at high temperatures.

[0141] (3) Organic solvent resistance

[0142] By comparing the relative enzyme activities of immobilized enzyme and free enzyme in different organic solvents ( Fig.12(c)) The tolerance of the two to organic solvents was explored. Free Sna and β-G and Sna&β-G@Cu / Fe-TADS(20) biocomposites were placed in different organic solvents (methanol, 99.5% ethanol, 99.5% n-butanol and 99.5% DMF) respectively. After incubation at room temperature for 6.5h, the enzyme activity of Sna&β-G@Cu / Fe-TADS(20) biocomposites hardly changed. However, the relative activity of the free enzyme showed a downward trend. Its relative enzyme activity in methanol, 99.5% ethanol, 99.5% n-butanol and 99.5% DMF was 83.5%, 89.8%, 86.2% and 84.2% of the initial enzyme activity, respectively. The main reason is that the secondary structure of the enzyme is easily changed in the organic solvent, resulting in a significant decrease in enzyme activity. However, compared with the free enzyme, Sna&β-G@Cu / Fe-TADS(20) biocomposites have an absolute advantage. The main reason is that Cu / Fe-TADS provides good physical protection for Sna and β-G, placing the enzyme in a relatively mild environment and protecting it from the corrosion of chemical denaturants, thereby improving the enzyme's tolerance to organic solvents.

[0143] (4) Storage stability

[0144] Storage stability is an important indicator for measuring the performance of immobilized enzymes. Therefore, the storage stability of free Sna and β-G and Sna&β-G@Cu / Fe-TADS(20) biocomposites at 4 °C was compared. The residual enzyme activity at different storage times was measured every 5 days ( Fig.12 (d)). The storage stability of free enzyme and immobilized enzyme for 30 days was evaluated. The results showed that the relative enzyme activity of Sna&β-G@Cu / Fe-TADS(20) biocomposite material remained basically unchanged after 30 days, while the relative enzyme activity of free Sna and β-G decreased by about 7%. The reason may be that Sna and β-G were fixed in the Cu / Fe-TADS carrier, which limited the change of the secondary structure of the enzyme, thereby effectively maintaining the relative activity of the enzyme.

[0145] 12. Effect of the scale-up preparation system on the performance of Sna&β-G@Cu / Fe-TADS

[0146] (1) Effect of relative enzyme activity and enzyme loading

[0147] The above characterization results show that the Sna&β-G@Cu / Fe-TADS biocomposite has good structural characteristics and stability. In order to further promote its scale-up production, this study investigated the effect of preparing Sna&β-G@Cu / Fe-TADS biocomposite within a 10-fold range on relative enzyme activity and enzyme loading. Fig.13In the process of the scaled-up preparation of Sna&β-G@Cu / Fe-TADS biocomposite, the enzyme loading was 159.58 mg / g, which was basically maintained at the level of the initial preparation system (20 mL). However, the relative enzyme activity of Sna&β-G@Cu / Fe-TADS biocomposite showed a downward trend as the preparation system was expanded.

[0148] (2) SEM image of the enlarged preparation system Sna&β-G@Cu / Fe-TADS

[0149] In order to explore the reason for the decrease in relative enzyme activity of Sna&β-G@Cu / Fe-TADS biocomposites during the scale-up preparation process, the SEM images of Sna&β-G@Cu / Fe-TADS biocomposites prepared under different systems were compared ( Fig.14 (a) to (f)). The results show that with the continuous expansion of the preparation system, the flower-like structure of the Sna&β-G@Cu / Fe-TADS biocomposite material is gradually destroyed, which hinders the effective contact between the enzyme and the substrate and the transfer of substances. Therefore, it is necessary to effectively solve the problem of MOF structure destruction caused by material transfer during the scale-up preparation process.

[0150] (3) SEM images of materials prepared under different conditions at different scales

[0151] Fig.15 (a) to (d) compare the SEM images of Cu / Fe-TADS loaded with and without enzyme in 20mL and 200mL systems at different scales (10um, 5um, 1um and 500nm). Fig.15 In (a), it can be seen that the Sna&β-G@Cu / Fe-TADS (20) biocomposite material exhibits a good flower-like structure and an obvious pore structure on the surface. The flower-like structure of the Sna&β-G@Cu / Fe-TADS (200) biocomposite material is relatively dense, which reduces the surface porosity and thus hinders the effective contact between the enzyme and the substrate. The Cu / Fe-TADS carrier without enzyme loading has a honeycomb structure. The results show that the addition of enzymes is beneficial to the formation of the flower-like structure of the Sna&β-G@Cu / Fe-TADS biocomposite material. The reason may be that the interaction between metal ions and the amino or carboxyl groups of proteins promotes the growth of the MOF carrier around the enzyme, which is more conducive to regulating the structure of the biocomposite material, thereby achieving the purpose of efficient conversion. Fig.15 As shown in (d), the apparent morphology of Cys-MOF (200) obtained in the enlarged preparation system has changed significantly. The reason may be that in the larger preparation system, there is no enzyme promotion effect, and the mass transfer resistance of the substance increases significantly.

[0152] 13. Comparative analysis of enzyme-catalyzed reaction kinetics

[0153] Table 4 compares the kinetic parameters of free Sna and β-G and Sna&β-G@Cu / Fe-TADS biocomposites. The results show that the catalytic rate of Sna&β-G@Cu / Fe-TADS biocomposites has a significant increase compared with the free enzyme, indicating that the increase in mesopores and macropores greatly promotes the material transfer rate. In addition, the catalytic efficiency of Sna&β-G@Cu / Fe-TADS biocomposites has been significantly improved, mainly because the flower-like structure is conducive to the exposure of the enzyme active site and promotes the effective contact between the enzyme and the substrate.

[0154] Table 4 Kinetic parameters of free Sna, β-G and Sna&β-G@Cu / Fe-TADS biocomposites

[0155] Samples <![CDATA[V max (mM min) -1 )]]> <![CDATA[K m (mM)]]> <![CDATA[k cat / K m (mM -1 ·s -1 )]]> FreeSna&β-G 0.836 0.356 2.836 Sna&β-G@Cu / Fe-TADS 0.997 0.327 3.456

[0156] 14. Conversion efficiency of Sna&β-G@Cu / Fe-TADS at different conversion times

[0157] like Fig.16 As shown in the figure, with the extension of conversion time, the conversion rate and concentration of rare ginsenoside CK at 48h and 72h were 69.17% and 1.13mg / mL and 73.21% and 1.22mg / mL, respectively. At 24h, the conversion rate and concentration of rare ginsenoside CK did not increase significantly. Therefore, in order to balance the relationship between production cost and production efficiency, the optimal conversion time was determined to be 48h.

[0158] 15. Cyclic stability analysis

[0159] Recyclability is an important criterion for measuring the industrial feasibility and stability of biocomposites. The biocomposites that have completed the catalytic task can be recycled and reused by centrifugation or other methods. Fig.17 As shown in the figure, after the Sna&β-G@Cu / Fe-TADS biocomposite material was recycled for 6 times, the recovery rate could reach 60.25%, and the relative enzyme activity was maintained at 69.45% of the original enzyme activity. During the recycling process, the reasons for the decrease in the relative enzyme activity of the Sna&β-G@Cu / Fe-TADS biocomposite material may include three aspects. First, the shear force generated by the oscillation reaction during the conversion process caused the material to partially break and the enzyme to leak. Second, the continuous heating environment caused partial changes in the secondary structure of the enzyme. Third, during the conversion process, some substrates and products accumulated in the pores of the Sna&β-G@Cu / Fe-TADS biocomposite material during the recycling process, blocking the transport channel and reducing the mass transfer efficiency.

[0160] 16. Effect of the scale-up transformation system on CK conversion rate

[0161] By exploring the structural properties and conversion performance of the Sna&β-G@Cu / Fe-TADS biocomposite, we fully understand the application potential of this biocomposite. Therefore, in order to further promote its application in industrial production, this study explored the conversion rate and concentration of CK in the scaled-up conversion system. Fig.18 As shown in the figure, the conversion rate of rare ginsenoside CK in the 10-fold amplification conversion system was maintained at about 60%, and the concentration was 0.95 mg / mL. The results show that within this amplification conversion range, the Sna&β-G@Cu / Fe-TADS biocomposite material still exerted a good catalytic conversion effect. The reason for the decreasing trend in conversion rate may be that the laboratory conversion reaction conditions are limited, and there are restrictions on the control of conversion temperature and Sinian velocity.

[0162] 17. Sedimentation performance of Sna&β-G@Cu / Fe-TADS

[0163] (1) Recovery rate of Sna&β-G@Cu / Fe-TADS at different sedimentation times

[0164] Controlling production costs is a key factor in product production. In the process of promoting the industrial application of enzyme@MOF biocomposites, material recycling is crucial. Fig.19 As shown in (a) to (f), the Sna&β-G@Cu / Fe-TADS biocomposite material has obvious sedimentation with the extension of time. Therefore, the biocomposite material can be efficiently recovered by gravity sedimentation. By comparison, it was found that the sedimentation amount did not change significantly after 3 hours. Therefore, the optimal sedimentation recovery time of the Sna&β-G@Cu / Fe-TADS biocomposite material was determined to be 3 hours, and the recovery rate reached 88.25%.

[0165] (2) Effect of deposition recovery on the performance of Sna&β-G@Cu / Fe-TADS

[0166] The recovery of Sna&β-G@Cu / Fe-TADS biocomposites by sedimentation has good economic benefits. In order to further explore its industrial application potential, this study compared the effects of different sedimentation times on the relative enzyme activity and loading of Sna&β-G@Cu / Fe-TADS biocomposites. Fig. 20 As shown in the figure, with the increase of sedimentation time, the enzyme loading of Sna&β-G@Cu / Fe-TADS biocomposite was 156.25 mg / g, and the relative enzyme activity decreased by only 2% after 3 h. This further proves that Sna&β-G@Cu / Fe-TADS biocomposite has good application potential.

[0167] (3) SEM images of Sna&β-G@Cu / Fe-TADS at different sedimentation times

[0168] The recovery rate of Sna&β-G@Cu / Fe-TADS biocomposite can be further improved with the extension of sedimentation time. However, if the Sna&β-G@Cu / Fe-TADS biocomposite is placed in the reaction solution for a long time, it will continue to grow, thereby destroying the good conversion performance of the material due to its structural properties. Fig.21 As shown in (a) to (e), as the sedimentation time increases, the surface of the Sna&β-G@Cu / Fe-TADS biocomposite gradually loses the structural performance advantages of MOF, thereby reducing its catalytic conversion performance.

[0169] In summary, the present invention selects disodium terephthalate, an organic ligand with good water solubility, and introduces ferrous ions to prepare Sna&β-G@Cu / Fe-TADS containing hierarchical pores through a metal competition strategy for cascade catalysis of ginsenoside Rb1 to prepare rare ginsenoside CK. Its potential for industrial application was measured by exploring its structural properties, stability, catalytic conversion performance, and sedimentation recovery performance. The main conclusions are as follows:

[0170] (1) The replacement of sodium salt ligands successfully achieved the aqueous phase preparation of Sna&β-G@Cu / Fe-TADS biocomposites;

[0171] (2)Fe 2+ The hierarchical porous flower-like biocomposite with macropores was successfully prepared by the oxidation and competitive coordination of

[0172] (3) After 3 h of physical sedimentation, the recovery rate of Sna&β-G@Cu / Fe-TADS biocomposite reached 88.25%;

[0173] (4) Under the optimal conversion conditions, the concentration and conversion rate of rare ginsenoside CK in Sna&β-G@Cu / Fe-TADS biocomposite material reached 1.13 mg / mL and 69.75%, respectively.

[0174] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0175] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores, characterized in that: The following steps are involved: Under stirring conditions, snail enzyme and β-glycosidase were mixed with sodium deoxycholate solution, and then Cu 2+ Aqueous solution and Fe 2+ aqueous solution, encapsulating snail enzyme and β-glycosidase in Cu / Fe-NaDC hydrogel, keeping the enzyme protein structure intact, and generating Sna&β-G@Cu / Fe-NaDC hydrogel; Under stirring conditions, an organic ligand disodium terephthalate is added to the Sna&β-G@Cu / Fe-NaDC hydrogel, and the organic ligand captures the metal ions in the hydrogel, and a Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores is prepared through oxidation and metal competitive coordination.

2. The method for preparing the Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores according to claim 1, characterized in that: Sodium deoxycholate, Cu 2+ , the molar ratio of disodium terephthalate is 1:2:0.5~1.

3. The method for preparing the Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores according to claim 1, characterized in that: Cu 2+ with Fe 2+ The molar ratio is 1:

1.

4. The method for preparing the Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores according to claim 1, characterized in that: The magnetic stirring time was 0.5 h when preparing the hydrogel, and the magnetic stirring time was 3 h when preparing the composite material.

5. The method for preparing the Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores according to claim 1, characterized in that: The ratio of the amount of snail enzyme and β-glycosidase added to the amount of sodium deoxycholate solution was 50 mg:5 mL, wherein the concentration of the sodium deoxycholate solution was 29 mg / mL.

6. The method for preparing the Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores according to claim 1, characterized in that: The mass ratio of snailase to β-glycosidase was 49.752:0.

248.

7. The method for preparing the Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores according to claim 1, characterized in that: The Cu 2+ The aqueous solution is copper acetate solution, Fe 2+ The solution is ferrous acetate solution.

8. The method for preparing the Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores according to claim 7, characterized in that: The molar ratio of the ferrous acetate solution to disodium terephthalate is 1:

2.

9. A Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores obtained by the preparation method according to any one of claims 1 to 8.

10. An application of the Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores as claimed in claim 9 in catalytic conversion of ginsenosides, characterized in that: The Sna&β-G@Cu / Fe-TADS biocomposite material with hierarchical pores is used to catalytically transform ginsenoside Rb1 to prepare ginsenoside CK.