Method for regulating and controlling Laves phase of additive manufacturing nickel-based superalloy
By using interlayer deformation composite technology in additive manufacturing nickel-based high-temperature alloys, the formation of Laves phase and the precipitation of reinforced phases are controlled, and the problems of material strength reduction and easy fracture caused by Laves phase are solved, and the mechanical properties of the material are improved.
Patent Information
- Application Number
- CN202411030583.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
During the additive manufacturing process, the formation of the Laves phase in nickel-based high-temperature alloy leads to reduced material strength and easy breakage, and the prior art is difficult to effectively reduce its content and size, and the impact of traditional methods on the strengthened phase γ" phase is not obvious.
Through interlayer deformation composite additive manufacturing technology, it includes interlayer plastic deformation processing and adjusting heat input parameters during laser deposition, controlling the grain recrystallization ratio, reducing the Laves phase content and promoting the precipitation of the enhanced phase γ” phase.
It effectively reduces the content and size of the Laves phase, increases the content of strengthening elements in the matrix, promotes the formation of the strengthening phase γ" phase, and improves the mechanical properties of the material.
Smart Images

Figure CN118957333A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal material composite additive manufacturing, and in particular to a method for regulating and controlling Laves phase in additive manufacturing of nickel-based high-temperature alloys. Background Art
[0002] Additive manufacturing technology, also known as "3D printing", is a process of directly forming three-dimensional solid parts by layering the digital data of the three-dimensional model and then using the processing method of "layered processing and layer-by-layer accumulation". Laser directed energy deposition is one of the methods of additive manufacturing, which processes parts by feeding metal powder into a laser-melted molten pool. The metal powder melts and solidifies rapidly under the action of high-energy lasers, and the microstructure is dense and uniform, and the formed parts have good mechanical properties. Due to the large heat input of the laser, it is convenient to process materials with high melting points and difficult to process. However, there is serious element segregation behavior in the solidification process of laser deposition. The strengthening elements Nb and Mo show high solid solubility in the liquid phase, so a large number of Nb and Mo atoms are enriched in the residual liquid phase, which eventually leads to the formation of long-chain Laves phases between dendrites. The formation of Laves phase consumes the strengthening elements in the matrix, thereby reducing the strength of the matrix and inhibiting the precipitation of the strengthening phase γ” phase. At the same time, the chain-like Laves phase easily serves as a path for crack propagation, making the formed part prone to fracture. Therefore, reducing the content of Laves phase and reducing its size are effective ways to improve material properties. In the traditional method, the cooling rate and temperature gradient in the additive process are usually controlled to affect the formation of Laves phase. Document 1 (CN202110864041) reduces element segregation and reduces the volume fraction of Laves phase by increasing the solidification rate of the molten pool during laser deposition, but its effect on the content of Laves phase is not obvious and does not promote the generation of the strengthening phase γ” phase. Document 2 (CN 114799204 A) reduces the content of Laves phase in additively manufactured high-temperature alloys by mixing nano-carbon powder with high-temperature alloy powder, but the addition of carbon element will generate a large amount of continuously distributed carbides, which will have an adverse effect on the plasticity of the material. Summary of the invention
[0003] In view of the shortcomings of the prior art, the present invention provides a method for regulating the Laves phase of a nickel-based high-temperature alloy in additive manufacturing; a method for reducing the Laves phase content and strengthening the precipitation phase through interlayer deformation composite additive manufacturing can improve the mechanical properties of the formed part.
[0004] A method for regulating Laves phase in additively manufactured nickel-based high-temperature alloys, comprising the following steps:
[0005] Step 1: Grind the substrate to remove the oxide film and clean it with an alkaline solution, dry the metal powder and put it into the powder feeder;
[0006] Step 2: 3D model the specimen to be printed, slice and trace the model, and import the generated trajectory planning program into the additive manufacturing system;
[0007] Step 3: Performing single-layer additive deposition;
[0008] Step 4: Perform interlayer plastic deformation treatment on the surface of the deposited layer so that the deposited layer reaches the required deformation amount;
[0009] Step 5: After the deposited layer that has undergone interlayer plastic deformation treatment cools down to room temperature, additive deposition is continued on its surface;
[0010] Step 6: Alternate additive deposition and interlayer plastic deformation to ultimately obtain a formed part with a reduced Laves phase content.
[0011] The method for controlling the Laves phase of a nickel-based high-temperature alloy in additive manufacturing, the influence depth H of the interlayer plastic deformation in step 4 D Need to meet
[0012] H D >H R +H A
[0013] Where H D is the influence depth of interlayer plastic deformation, that is, the work hardening depth caused by the single-layer plastic deformation process, H R H is the remelting depth, that is, the depth to which the previous layer is remelted when a new layer is deposited. A is the average layer thickness after plastic deformation;
[0014] The method for controlling the Laves phase of the additively manufactured nickel-based high-temperature alloy, in step 5, is H away from the bottom of the molten pool. A The temperature T at which the R When T<T R When T R is the critical recrystallization temperature, T is the distance from the bottom of the molten pool A The temperature at in, is the net input power, α is the thermal diffusion coefficient, T s is the heat source moving speed, T0 is room temperature, C p is the specific heat capacity, t is the wall thickness, K0() is the zero-order Bessel function of the first kind;
[0015] The method for regulating Laves phase in additive manufacturing of nickel-based high-temperature alloys, in the additive deposition process in step 5, the heat input is controlled by adjusting the input power and the heat source movement speed during the additive deposition process, thereby controlling the proportion of recrystallization of grains and the content of Laves phase in the additive manufacturing sample;
[0016] The method for regulating the additive manufacturing of Laves phase of nickel-based high-temperature alloy, the interlayer plastic deformation process includes interlayer hammering, interlayer rolling and interlayer ultrasonic shot peening, and the equipment for generating interlayer plastic deformation includes air hammer, hydraulic press and electromagnetic hammer;
[0017] The method for regulating and additively manufacturing Laves phase of nickel-based high-temperature alloy, wherein the heat source for additive deposition includes laser, arc, electron beam and ion beam.
[0018] The beneficial effects of adopting the above technical solution are:
[0019] The present invention provides a method for regulating the Laves phase of a nickel-based high-temperature alloy in additive manufacturing. A large amount of mechanical energy is introduced during the laser deposition process through interlayer deformation, so that the Laves phase is fragmented and a large number of dislocations are generated inside the material. The size of the fragmented Laves phase is reduced, making it easier to dissolve. At the same time, the generation of dislocations provides more diffusion channels for Nb atoms, making it easier for Nb atoms to diffuse. In the subsequent layer deposition heat input process, recrystallization occurs with the subgrains formed by dislocation entanglement as the core. The recrystallization process is accompanied by the migration of grain boundaries, which further promotes the dissolution of the Laves phase back into the matrix. The large amount of Laves phase back into the matrix promotes the increase of the strengthening element Nb content in the matrix. At the same time, interlayer deformation introduces a large number of dislocations. The aggregation of Nb near the dislocations promotes the in-situ precipitation of the γ" phase under the action of the subsequent layer additive manufacturing cycle heat input. Interlayer deformation not only reduces the content of the Laves phase, but also reduces the size of the residual Laves phase, and at the same time promotes the formation of the strengthening phase γ" phase, thereby improving the mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of an interlayer deformation composite additive manufacturing device in an embodiment of the present invention.
[0021] Figure 2 Schematic diagram of the evolution principle of precipitation phase during interlayer deformation composite additive manufacturing in an embodiment of the present invention.
[0022] Figure 3 The microstructure morphology and precipitated phase content of the interlayer deformation composite additive manufacturing specimen in the embodiment of the present invention. DETAILED DESCRIPTION
[0023] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0024] The specific implementation steps are as follows:
[0025] (1) Figure 1 The figure is a schematic diagram of the interlayer deformation composite additive manufacturing device. In the embodiment, interlayer hammering composite laser directional energy deposition is used to perform composite manufacturing of GH4169. The optimal laser process parameters are determined as follows: laser power P = 1800w, laser speed of 0.01m / s, powder feeding rate of 15g / min, and argon as protective gas. After drying, the GH4169 powder is placed in the powder feeder for laser deposition additive manufacturing.
[0026] (2) After the laser deposits a single layer, wait for the specimen to cool to room temperature and then use an air hammer as an interlayer plastic deformation device to perform interlayer hammer deformation on the deposited part. The air hammer head moves along a set trajectory in a single path under the control of the robot and acts on the top of the deposited layer in the form of pulses. The distance from the hammer head to the specimen surface is 10 mm, the moving rate of the hammer head is 2 mm / s, and two hammer strikes are performed. The hardness of the specimen is measured and observed by a hardness tester and an optical microscope to obtain H D =2.9mm, H R =2.3mm.
[0027] (3) Laser deposition is performed on the hammered surface, and in the subsequent process, air hammering and laser deposition are performed alternately to finally complete the manufacture of the specimen. The thickness of the specimen is t = 5 mm, and the average layer thickness is H A =0.4mm, satisfying H D >H R +H A The parameter values described in Summary of the Invention 4 are: C p =657.2(J / (Kg·℃)), t=5mm, H A =0.4mm, T s =0.01m / s, α=1.1(㎡ / s), T0=25℃, T R =910℃, from which we can calculate T = 697.7℃ <T R , the grains partially recrystallize. Schematic diagram of the evolution of precipitation phase during interlayer deformation composite additive manufacturing, as shown in Figure 2 shown.
[0028] (4) The interlaminar hammering specimens obtained in this example were subjected to microstructure testing, such as Figure 3The sample shown is an alternating distribution of non-recrystallized areas and recrystallized areas, wherein the Laves phase contents in the non-recrystallized area and the recrystallized area are 0.47% and 0.26% respectively, and the Laves phase content in the sample obtained by deposition alone is 1.15%, indicating that the interlayer hammering process significantly reduces the Laves phase content. The above description is only a preferred embodiment of the present disclosure and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the embodiments of the present disclosure is not limited to the technical solutions formed by the specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the above-mentioned inventive concept. For example, the above-mentioned features are replaced with the technical features with similar functions disclosed in the embodiments of the present disclosure (but not limited to).
Claims
1. A method for regulating Laves phase in additively manufactured nickel-based high-temperature alloys, characterized in that: The following steps are involved: Step 1: Grind the substrate to remove the oxide film and clean it with an alkaline solution, dry the metal powder and put it into the powder feeder; Step 2: 3D model the specimen to be printed, slice and trace the model, and import the generated trajectory planning program into the additive manufacturing system; Step 3: Performing single-layer additive deposition; Step 4: Perform interlayer plastic deformation treatment on the surface of the deposited layer so that the deposited layer reaches the required deformation amount; Step 5: After the deposited layer that has undergone interlayer plastic deformation treatment cools down to room temperature, additive deposition is continued on its surface; Step 6: Alternate additive deposition and interlayer plastic deformation to ultimately obtain a formed part with a reduced Laves phase content.
2. The method for controlling Laves phase in additive manufacturing of nickel-based high-temperature alloy according to claim 1, characterized in that: The influence depth H of the interlayer plastic deformation described in step 4 D Need to meet H D >H R +H A Where H D is the influence depth of interlayer plastic deformation, that is, the work hardening depth caused by the single-layer plastic deformation process, H R H is the remelting depth, that is, the depth to which the previous layer is remelted when a new layer is deposited. A is the average layer thickness after plastic deformation.
3. The method for controlling Laves phase in additive manufacturing of nickel-based high-temperature alloy according to claim 1, characterized in that: In step 5, the distance from the bottom of the molten pool is H A The temperature T at which the R When T<T R When T R is the critical recrystallization temperature, T is the distance from the bottom of the molten pool A The temperature at in, is the net input power, α is the thermal diffusion coefficient, T s is the heat source moving speed, T0 is room temperature, C p is the specific heat capacity, t is the wall thickness, and K0() is the zero-order Bessel function of the first kind.
4. The method for controlling Laves phase in additive manufacturing of nickel-based high-temperature alloy according to claim 1, characterized in that: During the additive deposition process in step 5, the heat input is controlled by adjusting the input power and the heat source moving speed during the additive deposition process, thereby controlling the proportion of recrystallization of grains and the content of Laves phase in the additively manufactured sample.
5. The method for controlling Laves phase in additive manufacturing of nickel-based high-temperature alloy according to claim 1, characterized in that: The interlayer plastic deformation process includes interlayer hammering, interlayer rolling and interlayer ultrasonic shot peening, and the equipment for generating interlayer plastic deformation includes air hammer, hydraulic press and electromagnetic hammer.
6. The method for controlling Laves phase in additive manufacturing of nickel-based high-temperature alloy according to claim 1, characterized in that: The heat sources for additive deposition include laser, arc, electron beam and ion beam.
Citation Information
Patent Citations
Method for inhibiting Laves phase precipitation in nickel-based alloy laser additive manufacturing process
CN113579249A
Method for reducing brittle Laves phase in laser additive manufacturing nickel-based superalloy and improving strength and plasticity
CN114799204A
Method for controlling brittleness Laves phases in laser additive manufacturing process of nickel-based high-temperature alloy
CN106077647A
Method for refining additive manufactured titanium alloy grains
CN109128172A
Synchronous hammering shape control device and method for metal component additive manufacturing
CN113145861A