Zinc-aluminum-magnesium coating material and preparation method thereof
By using a cored induction electric furnace and a spiral mixer in the production of zinc-aluminum-magnesium alloy, combined with nitrogen injection and optimized cooling methods, the problems of oxide inclusion and gauge defects in zinc-aluminum-magnesium alloy are solved, and the product is improved Quality and production efficiency.
Patent Information
- Application Number
- CN202410945000.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-15
AI Technical Summary
Existing zinc-aluminum-magnesium alloys are prone to oxide inclusions, element segregation, and gauge defects during the production process, resulting in low product quality and difficult to meet the quality requirements of high-end galvanized products.
Core-based induction furnace for melting and casting, combined with spiral mixer and nitrogen injection technology, optimize the addition method of refining agent, adopt single-use casting and multiple cooling methods to control the temperature and cooling speed of the alloy melt to reduce oxides Inclusions and gauge defects.
It significantly reduces the incidence of oxide inclusions and gauge defects, improves the quality and utilization of zinc-aluminum-magnesium alloys, shortens production time, reduces costs, and ensures high quality and efficient production of products.
Smart Images

Figure CN118957359A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal smelting, and in particular to a zinc-aluminum-magnesium coating material and a preparation method thereof. Background Art
[0002] Hot-dip galvanizing is the most widely used and most cost-effective steel surface treatment method, and is widely used in the fields of automobiles, construction, home appliances, chemicals, machinery, petroleum, metallurgy, light industry, transportation, electricity, aviation and marine engineering. In recent years, zinc-aluminum-magnesium alloy-coated steel has become a high-value-added short-term product supported and developed with priority by the state, but zinc-aluminum-magnesium-coated products, especially thick plate and thick zinc layer products such as photovoltaic brackets, are prone to zinc flow lines, black spots, oxide inclusions and other problems during the production process, which has seriously restricted its development and promotion and application in the field of high-end galvanized products.
[0003] With the adjustment of the production capacity structure of hot-dip galvanized steel in my country and the increasingly high requirements for steel anti-corrosion, especially the more stringent requirements for the galvanizing quality of high-end galvanized products, the quality requirements for hot-dip galvanized alloys are getting higher and higher. How to control the internal oxide inclusions of zinc-aluminum-magnesium alloys, and how to inhibit and eliminate element segregation, physical defects, internal shrinkage cavities and other problems have become difficult problems faced by many zinc-aluminum-magnesium alloy manufacturers.
[0004] The existing smelting methods and smelting methods of zinc-aluminum-magnesium alloys require high smelting temperatures and high casting temperatures during the smelting process, and the temperature gradient is large, and metal elements are prone to uneven alloying. In addition, when adding more active metals such as magnesium, rare earth and other alloying elements, overburning is prone to occur, oxide slag inclusions are difficult to control, the slag rate of product production is high, and the utilization rate of valuable metals is low. At the same time, element segregation, shrinkage cavities at the bottom of the alloy, internal shrinkage cavities, fish scale patterns, cracks and other physical defects are also generated, which is not conducive to the production of high-quality products.
[0005] Therefore, there is an urgent need to explore an efficient zinc-aluminum-magnesium alloy smelting method to effectively reduce the oxide inclusions in the zinc-aluminum-magnesium alloy and improve the quality of the zinc-aluminum-magnesium alloy products. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a zinc-aluminum-magnesium coating material with less oxide inclusions and high alloy quality and a preparation method thereof.
[0007] In order to solve the above technical problems, the present invention provides a zinc-aluminum-magnesium coating material, which comprises, by mass percentage, 5%-8% Al, 1.5%-3.0% Mg, 0.01%-0.06% lanthanum-cerium mixed rare earth,
[0008] 0.05%-0.2%Si, 0.005%-0.02%B, 0.015%-0.1%Ti, 0.01%-0.06%Sr,
[0009] 0.01%-0.08% Ca, the balance is Zn and inevitable impurities.
[0010] The present invention also provides a method for preparing a zinc-aluminum-magnesium coating material, comprising the following steps:
[0011] The metal raw materials include 5%-8% Al, 1.5%-3.0% Mg, 0.01%-0.06% lanthanum-cerium mixed rare earth, 0.05%-0.2% Si, 0.005%-0.02% B, 0.015%-0.1% Ti, 0.01%-0.06% Sr, 0.01%-0.08% Ca, and the balance is Zn and unavoidable impurities: zinc ingot, aluminum ingot, magnesium ingot, aluminum-titanium-boron alloy, aluminum-silicon alloy, zinc-aluminum rare earth alloy, aluminum-calcium alloy and aluminum-strontium alloy;
[0012] After the zinc ingot and the aluminum ingot are added into the core induction furnace for melting, aluminum-titanium-boron alloy, aluminum-silicon alloy, zinc-aluminum rare earth alloy, aluminum-calcium alloy and aluminum-strontium alloy are added at 520-560°C, and after smelting, the first part of the refining agent is added to slag, slag pounding and slag raking to obtain the zinc-aluminum molten liquid;
[0013] Add magnesium ingots to the zinc-aluminum molten liquid in batches, and continue stirring for 20 to 40 minutes after smelting to obtain the zinc-aluminum-magnesium molten liquid;
[0014] The second part of the refining agent is sprayed into the lower part of the zinc-aluminum-magnesium melt through the nitrogen adding pipe by high-pressure nitrogen to form slag. After the refining agent spraying is completed, the nitrogen is continuously introduced for 5 to 15 minutes, and then the slag is allowed to stand for 15 to 25 minutes to slag, rake the slag and detect the composition of the zinc-aluminum-magnesium alloy melt;
[0015] The zinc-aluminum-magnesium alloy melt is cast at one time, the temperature is 520-560℃, the mold temperature is not more than 70℃, and the surface slag is removed after casting;
[0016] After casting is completed, when the cooling and solidification area of the casting blank is ≥90%, a cover plate is added or water is poured to form an alloy ingot;
[0017] The mold and the surface of the alloy ingot are cooled by fan or / and water injection to forcefully cool the mold and the surface of the alloy ingot, so that the alloy ingot is completely solidified to obtain a zinc-aluminum-magnesium alloy ingot.
[0018] Furthermore, a spiral mixer is arranged in the furnace body of the core induction furnace.
[0019] Furthermore, when the magnesium ingots are added to the zinc-aluminum melt in batches, each added magnesium ingot is pressed into the zinc-aluminum melt.
[0020] Furthermore, the total mass of the refining agent is 0.6% to 1% of the total mass of the metal raw material, the first part of the refining agent is 55 to 65% of the total mass of the refining agent, and the second part of the refining agent is 35 to 45% of the total mass of the refining agent.
[0021] Furthermore, the refining agent is a low-fluorine and chlorine refining agent including charcoal powder, silicon dioxide and river sand.
[0022] Furthermore, the cored induction furnace discharges the obtained zinc-aluminum-magnesium alloy melt from the bottom of the furnace body.
[0023] Furthermore, the zinc-aluminum-magnesium alloy melt enters the casting mold by blocking the chute with refractory bricks during one-time casting, and the chute is cleaned after casting.
[0024] Furthermore, when the casting blank is watered to form the initial alloy ingot, water is injected at a flow rate of less than 0.1 m / s in the middle of the casting blank to cool it, and water is sprayed at the edge of the mold to cool the mold temperature.
[0025] Furthermore, during the process of completely solidifying the alloy ingot to obtain the zinc-aluminum-magnesium alloy ingot, a small water column injection cooling or spray cooling with a water flow rate of less than 0.1 m / s is adopted, and the water is controlled to flow from the edge of the mold to the middle of the alloy ingot during water injection. The water is continuously injected for cooling at one time so that the water covers the alloy ingot, and the cooling time is 20-30 minutes.
[0026] The invention provides a zinc-aluminum-magnesium coating material, which has less oxide inclusions and higher product quality.
[0027] The present invention provides a method for preparing a zinc-aluminum-magnesium coating material, which uses a cored induction furnace to produce aluminum-zinc-aluminum-magnesium alloy, and can be smelted and cast at 520-560°C, thereby reducing the temperature of alloy smelting and casting, overcoming the problem of element burnout caused by the current use of a reverberatory furnace with an open flame to directly burn the surface of zinc liquid, and having a high utilization rate of valuable metals and few oxide inclusions. In addition, the furnace body of the cored induction furnace used in the present invention is itself equipped with a spiral stirrer, which has a high mechanical stirring intensity, and the metals such as Al, Mg, Ti, and Sr that can be added are easy to melt, the number of refractory and easily oxidizable metal inclusions in the alloy liquid is significantly reduced, and the alloy liquid has a uniform composition. At the same time, the cored induction furnace body of the present invention adopts a bottom discharge method for the smelted alloy liquid, which can overcome the impact oxidation of the alloy liquid caused by the impact of the alloy liquid during the tilting and casting process of the coreless induction furnace, solve the problem of air absorption oxidation during the alloy liquid melting and casting process, and reduce the generation of inclusions in the alloy.
[0028] In addition, the preparation method of a zinc-aluminum-magnesium coating material provided by the present invention changes the adding method of the refining agent, optimizes the traditional surface slag making process, adopts the method of combining nitrogen + refining agent and introducing it from the bottom of the zinc liquid for mixed slag making, and purging with nitrogen for 5 to 15 minutes, which can effectively promote the precipitation of suspended matter such as oxide inclusions that are not easy to precipitate in the alloy melt during the smelting process. At the same time, by letting the alloy melt stand for 15 to 25 minutes after the slag making is completed, the Fe-containing phase in the melt can be effectively precipitated, thereby improving the quality of the final zinc-aluminum-magnesium alloy ingot product.
[0029] In addition, the preparation method of the zinc-aluminum-magnesium coating material provided by the present invention adopts one-time casting, assisted by air cooling and water cooling, etc., replacing the secondary casting and multiple casting methods, shortening the operation time and reducing the production cost.
[0030] At the same time, the present invention provides a method for preparing a zinc-aluminum-magnesium coating material. After casting is completed, wait for the surface to slowly cool and solidify to a certain extent, add a cover plate before the block fish scale pattern appears on the ingot surface, or use a small water column with a water flow rate of less than 0.1m / s for water injection cooling or spray cooling, that is, when the area of the surface of the casting blank to be cooled and solidified is ≥90%, sprinkle a small amount of water near the middle position of the casting ingot. By using water for strong cooling, the last small volume of molten alloy can be quickly solidified and crystallized, avoiding the block fish scale pattern on the ingot surface. And, after the initial alloy ingot is formed, continue to use a fan to cool or sprinkle water on the edge of the mold to cool the mold temperature, so that the initial alloy ingot is crystallized and solidified in an orderly manner from the bottom and side to the middle and upper part, avoiding cracks and shrinkage holes on the surface of the alloy ingot due to insufficient cooling speed. Through the above cooling method, the surface physical specifications of the obtained zinc-aluminum-magnesium alloy ingot can be significantly improved, and the surface physical specification qualification rate of the obtained zinc-aluminum-magnesium alloy ingot can be above 96%. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A flow chart of a method for preparing a zinc-aluminum-magnesium coating material provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0032] See also Figure 1 The present invention provides a method for preparing a zinc-aluminum-magnesium coating material, comprising the following steps:
[0033] Step 1) Prepare metal raw materials in percentage by mass, including 5%-8% Al, 1.5%-3.0% Mg, 0.01%-0.06% lanthanum-cerium mixed rare earth, 0.05%-0.2% Si, 0.005%-0.02% B, 0.015%-0.1% Ti, 0.01%-0.06% Sr, 0.01%-0.08% Ca, and the balance is Zn and unavoidable impurities. The metal raw materials include zinc ingots, aluminum ingots, magnesium ingots, aluminum-titanium-boron alloys, aluminum-silicon alloys, zinc-aluminum rare earth alloys, aluminum-calcium alloys and aluminum-strontium alloys.
[0034] Among them, the mass ratio of aluminum, titanium and boron in aluminum-titanium-boron alloy is 95:1:4, the mass ratio of aluminum to silicon in aluminum-silicon alloy is 11:89, the mass ratio of zinc, aluminum and rare earth in zinc-aluminum rare earth alloy is 20:2:78, the mass ratio of aluminum to calcium in aluminum-calcium alloy is 8:2, and the mass ratio of aluminum to strontium in aluminum-strontium alloy is 95:5.
[0035] Step 2) After the zinc ingot and the aluminum ingot are melted in a cored induction furnace, the temperature is raised to 520-560°C, and aluminum-titanium-boron alloy, aluminum-silicon alloy, zinc-aluminum rare earth alloy, aluminum-calcium alloy, and aluminum-strontium alloy are added in batches. After the metal is completely smelted, the first part of the refining agent is added, stirred evenly to allow it to react fully, and surface slag is formed. After manual slagging, the surface slag is removed to obtain a zinc-aluminum molten liquid.
[0036] Among them, a core induction furnace is used to produce aluminum-zinc-aluminum-magnesium alloy, which can be smelted at 520-560°C, reducing the alloy smelting temperature and overcoming the problem of element burnout caused by the current use of a reverberatory furnace with an open flame to directly burn the zinc liquid surface. The utilization rate of valuable metals is high and oxide inclusions are less.
[0037] In addition, the furnace body of the core induction furnace is equipped with a spiral stirrer, which has a high mechanical stirring intensity. The added metals such as Al, Mg, Ti, Sr, etc. are easily melted, the number of refractory and easily oxidized metal inclusions in the alloy liquid is significantly reduced, and the alloy liquid composition is uniform.
[0038] Step 3) adding magnesium ingots to the zinc-aluminum molten liquid in batches, and continuing to stir for 20 to 40 minutes after smelting to obtain a zinc-aluminum-magnesium molten liquid.
[0039] Among them, when adding magnesium ingots to the zinc-aluminum molten liquid in batches, add magnesium ingots in batches and adhere to the principle of small amounts and multiple times. After the metal magnesium ingot is completely smelted, continue stirring for 20 to 40 minutes. At the same time, in the process of adding magnesium ingots to the zinc-aluminum molten liquid, the magnesium ingot should be pressed into the zinc-aluminum molten liquid to avoid magnesium suspended on the surface of the zinc bath causing element burning and oxidation.
[0040] Step 4) The second part of the refining agent is sprayed into the lower part of the zinc-aluminum-magnesium melt through the nitrogen adding tube to form slag. After the refining agent is sprayed, the nitrogen is continued to be introduced for 5 to 15 minutes to promote the complete separation of suspended matter in the melt. Then the nitrogen adding tube is removed, and the zinc-aluminum-magnesium melt is allowed to stand for 15 to 25 minutes to promote the complete separation of Fe-containing phases in the melt. The slag is then manually pounded and raked, and finally the zinc-aluminum-magnesium alloy melt is sampled for component detection. When the composition of the zinc-aluminum-magnesium alloy melt sample meets the quality requirements, the next step of casting process is carried out.
[0041] In this process, the present invention changes the way of adding the refining agent, optimizes the traditional surface slag making process, adopts the method of combining nitrogen + refining agent and introducing it from the bottom of the zinc liquid for mixed slag making, and by purging with nitrogen for 5 to 15 minutes, it can effectively promote the full precipitation of suspended matter such as oxide inclusions that are not easy to precipitate in the alloy melt during the smelting process. At the same time, by letting the alloy melt stand for 15 to 25 minutes after the slag making is completed, it can effectively promote the full precipitation of Fe-containing phases in the melt, thereby improving the quality of the final zinc-aluminum-magnesium alloy ingot product.
[0042] In the whole process of smelting and slag making, the total mass of the refining agent added is 0.6% to 1% of the total mass of the metal raw material, wherein the first part of the refining agent added is 55 to 65% of the total mass of the refining agent, and the second part of the refining agent added is 35 to 45% of the total mass of the refining agent.
[0043] The refining agent is a low-fluorine and chlorine refining agent including charcoal powder, silicon dioxide and river sand.
[0044] Step 5) Casting the zinc-aluminum-magnesium alloy melt in one go, the temperature is 520-560° C., the mold temperature is not greater than 70° C., and after the casting is completed, the slag on the surface of the zinc-aluminum-magnesium alloy melt is removed.
[0045] The present invention adopts one-time casting, auxiliary cooling methods such as air cooling and water cooling, replacing the secondary casting or multiple casting methods, which can shorten the operation time, improve the process efficiency, thereby reducing the production cost and improving the economic benefit.
[0046] Furthermore, when the present invention discharges the zinc-aluminum-magnesium alloy melt in the cored induction furnace into the casting mold, the zinc-aluminum-magnesium alloy melt is directly discharged into the casting mold through the discharge port at the bottom of the cored induction furnace body.
[0047] The cored induction furnace body of the present invention adopts a bottom discharge method for the smelted alloy liquid, which can overcome the impact oxidation of the alloy liquid caused by the impact of the alloy liquid during the tilting and casting process of the coreless induction furnace, solve the problem of air absorption oxidation during the alloy liquid melting and casting process, and reduce the generation of inclusions in the alloy.
[0048] Meanwhile, the present invention uses refractory bricks to block the chute when the zinc-aluminum-magnesium alloy melt is cast in one go to enter the casting mold, which can reduce the sticky slag from entering the mold. After the casting is completed, the chute is cleaned in time.
[0049] Step 6) After the casting is completed, a cover plate is added or water is sprayed to form an initial alloy ingot when the cooling and solidification area of the cast blank is ≥ 90%.
[0050] When water is poured on the casting blank to form the initial alloy ingot, the water is poured in the middle of the casting blank, and water is poured on the edge of the mold to cool the mold temperature.
[0051] After the casting is completed, the surface is slowly cooled and solidified to a certain extent, and before block fish scale patterns appear on the ingot surface, a cover plate is added or a small water column with a water flow rate of less than 0.1 m / s is used for water injection cooling or spray cooling. That is, when the surface area of the cast blank to be cooled and solidified is ≥90%, a small water column with a water flow rate of less than 0.1 m / s is used for water injection cooling near the middle position of the casting ingot. By using strong water cooling, the last relatively small volume of molten alloy can be quickly solidified and crystallized, thereby avoiding the block fish scale patterns on the ingot surface.
[0052] Step 7) Use a fan to cool and / or inject water to forcefully cool the mold and the surface of the alloy ingot, so that the alloy ingot is completely solidified to obtain a zinc-aluminum-magnesium alloy ingot.
[0053] Among them, during the process of completely solidifying the alloy ingot to obtain the zinc-aluminum-magnesium alloy ingot, a small water column water injection cooling or spray cooling with a water flow rate below 0.1m / s is adopted, and the water is controlled to flow from the edge of the mold to the middle of the alloy ingot during water injection. The water is continuously injected for cooling at one time so that the water covers the alloy ingot, and the cooling time is 20-30min.
[0054] After forming the initial alloy ingot, the present invention continues to use a fan to cool the mold or spray water on the edge of the mold to cool the mold temperature, so that the initial alloy ingot is crystallized and solidified in an orderly manner from the bottom and side to the middle and upper part, avoiding cracks and shrinkage holes on the surface of the alloy ingot due to insufficient cooling speed. Through the above cooling method, the surface physical specifications of the obtained zinc-aluminum-magnesium alloy ingot can be significantly improved, and the surface physical specifications qualification rate of the obtained zinc-aluminum-magnesium alloy ingot can be above 96%.
[0055] The following is a specific description of the preparation method of the zinc-aluminum-magnesium coating material provided by the present invention through examples.
[0056] Example 1
[0057] A method for preparing a zinc-aluminum-magnesium coating material comprises the following steps:
[0058] The first step: according to the mass percentage of 5.9% Al, 2.1% Mg, 0.025% lanthanum-cerium mixed rare earth, 0.035% Si, 0.006% B, 0.03% Ti, 0.025% Sr, 0.025% Ca, the balance is Zn and unavoidable impurities, weigh zinc ingots, aluminum ingots, magnesium ingots, aluminum silicon alloy, zinc aluminum rare earth alloy, aluminum calcium alloy, aluminum strontium alloy, aluminum titanium boron alloy and other metal raw materials.
[0059] Step 2: Weigh out an environmentally friendly refining agent with a mass equivalent to 0.8% of the total mass of the metal raw materials in the first step.
[0060] Step 3: When the furnace temperature rises to 490°C, add the zinc ingots and aluminum ingots weighed in the first step into the core induction furnace, stir and smelt until they are completely melted.
[0061] Step 4: After the furnace temperature is raised to 520°C, add the intermediate alloys such as aluminum silicon alloy, zinc aluminum rare earth alloy, aluminum calcium alloy, aluminum strontium alloy, aluminum titanium boron alloy, etc. weighed in the first step in sequence, stir and smelt them completely, then add 60% of the total mass of the refining agent weighed in the second step, stir to make it fully react, and remove the slag on the surface of the melt.
[0062] Step 5: Add magnesium ingots in batches, 3.5 kg each time. Add magnesium ingots again after the last added magnesium ingot has melted. Press the magnesium ingot into the zinc liquid each time to prevent surface burning and oxidation. After all the magnesium ingots have melted completely, stir for 30 minutes.
[0063] Step 6: Add the remaining 40% refining agent to the alloy liquid to slag deep in the middle and bottom of the zinc liquid, and introduce nitrogen for 8 minutes to promote the precipitation of suspended matter in the melt. Let it stand for 20 minutes to promote the full precipitation of Fe-containing phase in the melt, and then rake the slag after manual slagging.
[0064] Step 7: Take samples to test aluminum, magnesium and impurity elements. If they do not meet the requirements, make adjustments until they meet the requirements before casting.
[0065] Step 8: Use one-time casting, control the temperature at 550℃±5℃, and the mold temperature is not more than 70℃.
[0066] Step 9: During the casting process, samples are taken from 2 / 6, 4 / 6, and 6 / 6 of the total number of ingots produced in each batch and inspected.
[0067] Step 10: After casting, wait for the surface to slowly cool and solidify to a certain degree. Before blocky fish scale patterns appear on the ingot surface, use a small water column injection cooling or spray cooling with a water flow rate below 0.1m / s to form an initial alloy ingot.
[0068] Step 11: After the initial alloy ingot is formed, use a fan to cool or inject water to forcefully cool the mold and the surface of the alloy ingot. Wait for the alloy ingot to completely cool and solidify to obtain a qualified product (i.e., zinc-aluminum-magnesium alloy ingot), demould, repair, batch number, inspect, and put into storage.
[0069] The zinc-aluminum-magnesium alloy ingot prepared in Example 1 of the present invention was tested and the main phase composition and proportion of the prepared zinc-aluminum-magnesium alloy ingot are shown in Table 1. The utilization rate of Mg and Si elements in the prepared zinc-aluminum-magnesium alloy ingot is shown in Table 2. The content of each component in the prepared zinc-aluminum-magnesium alloy ingot is shown in Table 3. The alloy remelting slag rate of the prepared zinc-aluminum-magnesium alloy ingot is shown in Table 4.
[0070] It can be seen from Table 1 that the shrinkage cavity and slag inclusion defects in the zinc-aluminum-magnesium alloy ingot prepared in the embodiment of the present invention are significantly improved, and the proportion of the alloy eutectic structure is increased.
[0071] It can be seen from Table 2 that the Si element utilization rate in the zinc-aluminum-magnesium alloy ingot prepared in the embodiment of the present invention is more than 90.3%, and the Mg element utilization rate reaches 95.30%, which is 8.3% higher than the Si element utilization rate of 82% in the reverberatory furnace, and 5.3% higher than the Mg element utilization rate of 90% in the reverberatory furnace.
[0072] It can be seen from Table 3 that the zinc-aluminum-magnesium alloy ingot prepared in the embodiment of the present invention has an Al segregation of ≤0.06%, a Mg segregation of ≤0.06%, a B segregation of ≤0.001%, a Ti segregation of ≤0.005%, and segregations of Si, Ca, Sr, and lanthanum-cerium mixed rare earth are all no more than 0.006%. Therefore, the segregation of various elements in the zinc-aluminum-magnesium alloy ingot prepared in the embodiment of the present invention is effectively controlled.
[0073] It can be seen from Table 4 that compared with the smelting in the reverberatory furnace, the smelting and casting temperatures of the embodiment of the present invention are reduced by 150-180° C., the production cost is significantly reduced, the slag production rate in the alloy casting process is reduced by 15%, and the product remelting slag rate is reduced by 0.46%.
[0074] Table 1
[0075]
[0076]
[0077] Table 2
[0078]
[0079] Table 3
[0080] batch 1 2 3 4 5 Al% 5.87 5.89 5.87 5.90 5.89 Mg% 2.10 2.08 2.12 2.06 2.08 Lanthanum-cerium mixed rare earth % 0.022 0.024 0.025 0.023 0.027 B% 0.0061 0.0064 0.0063 0.0063 0.0067 Ti% 0.032 0.035 0.036 0.033 0.037 Ca% 0.021 0.023 0.025 0.024 0.022 Si% 0.031 0.033 0.035 0.032 0.033 Sr% 0.021 0.022 0.025 0.022 0.023 Fe% 0.008 0.008 0.008 0.008 0.008 Pb% 0.0035 0.0036 0.0035 0.0037 0.0038 Cd% 0.002 0.0025 0.002 0.002 0.002 Cu% 0.002 0.002 0.002 0.002 0.002 Sn% <0.0005 <0.0005 <0.0005 <0.0005 <0.0005 V% - <0.002 <0.002 - -
[0081] Table 4
[0082]
[0083] The Fe content in the zinc-aluminum-magnesium alloy ingot prepared in the embodiment of the present invention is ≤0.008%, the oxide inclusions in the zinc-aluminum-magnesium alloy ingot are significantly reduced, the physical defects such as shrinkage cavities at the bottom of the alloy, internal shrinkage cavities, fish scales, cracks, etc. are significantly improved, and the product physical specification qualification rate reaches 96.4%.
[0084] Example 2
[0085] A method for preparing a zinc-aluminum-magnesium coating material comprises the following steps:
[0086] The first step: according to the mass percentage of Al: 5.75% Al, 2.06% Mg, 0.03% lanthanum-cerium mixed rare earth, 0.09% Si, 0.01% B, 0.05% Ti, 0.025% Sr, 0.025% Ca, the balance is Zn and unavoidable impurities, weigh zinc ingots, aluminum ingots, magnesium ingots, aluminum silicon alloy, zinc aluminum rare earth alloy, aluminum calcium alloy, aluminum strontium alloy, aluminum titanium boron alloy and other metal raw materials.
[0087] Step 2: Weigh a refining agent with a mass equivalent to 0.9% of the total mass of the metal raw materials in the first step.
[0088] Step 3: When the furnace temperature rises to 480°C, add the zinc ingots, aluminum ingots and other related alloys weighed in the first step into the core induction furnace and stir until they are completely melted.
[0089] Step 4: After the zinc and aluminum are melted, heat the mixture to 530°C, and add the aluminum-titanium-boron alloy, aluminum-silicon alloy, zinc-aluminum rare earth alloy, aluminum-calcium alloy, and aluminum-strontium alloy weighed in the first step in sequence. After sufficient stirring and smelting, add 60% of the total mass of the refining agent weighed in the second step, stir to allow for sufficient reaction, and remove the slag on the surface.
[0090] Step 5: Add magnesium ingots in batches, 4 kg each time. Add magnesium ingots again after the last added magnesium ingot has melted. Press the magnesium ingot into the zinc liquid after each addition to prevent surface burning and oxidation. Stir for 30 minutes after all the magnesium ingots have melted completely.
[0091] Step 6: Add the remaining 40% refining agent to the alloy liquid to slag deep in the middle and bottom of the zinc liquid, and introduce nitrogen for 8 minutes to promote the precipitation of suspended matter in the melt. Let it stand for 20 minutes to promote the full precipitation of Fe-containing phase in the melt, and then rake the slag after manual slagging.
[0092] Step 7: Raise the temperature and stir to homogenize the melt. Take samples to test aluminum, magnesium and impurity elements. If they do not meet the requirements, make adjustments until they meet the requirements before casting.
[0093] Step 8: Use one-time casting, control the temperature at 540℃±5℃, and the mold temperature is not more than 70℃.
[0094] Step 9: During the casting process, samples are taken and inspected from 1 / 6, 3 / 6, and 5 / 6 of the total number of ingots produced in each batch.
[0095] Step 10: After the casting is completed, the middle 2 / 3 of the surface area is immediately covered with a cover plate, and the surface is cooled and solidified to form an initial alloy ingot.
[0096] Step 11: After the initial alloy ingot is formed, use fan cooling / water injection to forcefully cool the mold and the surface of the alloy ingot. Wait for the alloy ingot to completely cool and solidify to obtain a qualified product (i.e., zinc-aluminum-magnesium alloy ingot), demould, repair, batch number, inspect, and put into storage.
[0097] The zinc-aluminum-magnesium alloy ingot prepared in Example 2 of the present invention was tested and the main phase composition and proportion of the prepared zinc-aluminum-magnesium alloy ingot are shown in Table 1. The utilization rate of Mg and Si elements in the prepared zinc-aluminum-magnesium alloy ingot is shown in Table 5. The content of each component in the prepared zinc-aluminum-magnesium alloy ingot is shown in Table 6. The alloy remelting slag rate of the prepared zinc-aluminum-magnesium alloy ingot is shown in Table 7.
[0098] It can be seen from Table 1 that the shrinkage cavity and slag inclusion defects in the zinc-aluminum-magnesium alloy ingot prepared in the embodiment of the present invention are significantly improved, and the proportion of the alloy eutectic structure is increased.
[0099] It can be seen from Table 5 that the Si element utilization rate in the zinc-aluminum-magnesium alloy ingot prepared in the embodiment of the present invention is 87.76%, and the Mg element utilization rate reaches 94.86%. The Si element utilization rate is equivalent to that of the coreless furnace, which is 2.86% higher than the Mg element utilization rate of 92% of the coreless furnace.
[0100] It can be seen from Table 6 that the zinc-aluminum-magnesium alloy ingot prepared in the embodiment of the present invention has Al segregation ≤0.06%, Mg segregation ≤0.05%, B segregation ≤0.004%, Ti segregation ≤0.008%, Si, Ca, Sr, and lanthanum-cerium mixed rare earth are all not more than 0.06%. Therefore, the segregation of various elements in the zinc-aluminum-magnesium alloy ingot prepared in the embodiment of the present invention is effectively controlled.
[0101] It can be seen from Table 7 that compared with the smelting in the reverberatory furnace, the smelting and casting temperatures of the embodiments of the present invention are reduced by 80-100° C., the production cost is significantly reduced, the slag production rate in the alloy casting process is reduced by 17%, and the product remelting slag rate is reduced by 0.65%.
[0102] Table 5
[0103]
[0104] Table 6
[0105]
[0106]
[0107] Table 7
[0108]
[0109] The Fe content in the zinc-aluminum-magnesium alloy ingot prepared in the embodiment of the present invention is ≤0.007%, the oxide inclusions in the zinc-aluminum-magnesium alloy ingot are significantly reduced, the physical defects such as shrinkage cavities at the bottom of the alloy, internal shrinkage cavities, fish scales, cracks, etc. are significantly improved, and the product physical specification qualification rate reaches 96.8%.
[0110] Example 3
[0111] A method for preparing a novel zinc-aluminum-magnesium coating material comprises the following steps:
[0112] The first step: according to the mass percentage of Al: 5.68%, Mg: 1.89%, lanthanum-cerium mixed rare earth: 0.025%, Si: 0.06%, B: 0.005%, Ti: 0.03%, Sr: 0.03%, Ca: 0.025%, the balance is Zn and unavoidable impurities, weigh zinc ingots, aluminum ingots, magnesium ingots, aluminum silicon alloy, zinc aluminum rare earth alloy, aluminum calcium alloy, aluminum strontium alloy, aluminum titanium boron alloy and other metal raw materials.
[0113] Step 2: Weigh a refining agent that is 1% of the total mass of the metal raw materials in the first step.
[0114] Step 3: When the furnace temperature rises to 480°C, add the zinc ingots, aluminum ingots and other related alloys weighed in the first step into the core induction furnace and stir until they are completely melted.
[0115] Step 4: After the zinc and aluminum are melted, heat the mixture to 530°C, and add the aluminum-titanium-boron alloy, aluminum-silicon alloy, zinc-aluminum rare earth alloy, aluminum-calcium alloy, and aluminum-strontium alloy weighed in the first step in sequence. After sufficient stirring and smelting, add 60% of the total mass of the refining agent weighed in the second step, stir to allow for sufficient reaction, and remove the slag on the surface.
[0116] Step 5: Add magnesium ingots in batches, 5 kg each time. Add magnesium ingots again after the last added magnesium ingot has melted. Press the magnesium ingot into the zinc liquid after each addition to prevent surface burning and oxidation. Stir for 30 minutes after all the magnesium ingots have melted completely.
[0117] Step 6: Add the remaining 40% refining agent to the alloy liquid to slag deep in the middle and bottom of the zinc liquid, and introduce nitrogen for 8 minutes to promote the precipitation of suspended matter in the melt. Let it stand for 20 minutes to promote the full precipitation of Fe-containing phase in the melt, and then rake the slag after manual slagging.
[0118] Step 7: Take samples to test aluminum, magnesium and impurity elements. If they do not meet the requirements, make adjustments until they meet the requirements before casting.
[0119] Step 8: Use one-time casting, control the temperature at 550-560°C, and the mold temperature is no more than 70°C.
[0120] Step 9: During the casting process, samples are taken and inspected from 1 / 6, 3 / 6, and 5 / 6 of the total number of ingots produced in each batch.
[0121] Step 10: After the casting is completed, the middle 2 / 3 of the surface of the casting blank is immediately covered with a cover plate, and the surface is allowed to cool and solidify to form an initial alloy ingot.
[0122] Step 11: After the initial alloy ingot is formed, use fan cooling / water injection to forcefully cool the mold and the surface of the alloy ingot. Wait for the alloy ingot to completely cool and solidify to obtain a qualified product (i.e., zinc-aluminum-magnesium alloy ingot), demould, repair, batch number, inspect, and put into storage.
[0123] The zinc-aluminum-magnesium alloy ingot prepared in Example 3 of the present invention was tested and the main phase composition and proportion of the prepared zinc-aluminum-magnesium alloy ingot are shown in Table 1. The content of each component in the prepared zinc-aluminum-magnesium alloy ingot is shown in Table 8. The alloy remelting slag rate of the prepared zinc-aluminum-magnesium alloy ingot is shown in Table 9.
[0124] It can be seen from Table 1 that the shrinkage cavity and slag inclusion defects in the zinc-aluminum-magnesium alloy ingot prepared in the embodiment of the present invention are significantly improved, and the proportion of the alloy eutectic structure is increased.
[0125] It can be seen from Table 8 that the zinc-aluminum-magnesium alloy ingot prepared in the embodiment of the present invention has Al segregation ≤0.06%, Mg segregation ≤0.05%, B segregation ≤0.006%, Ti segregation ≤0.008%, and Si, Ca, Sr, and lanthanum-cerium mixed rare earth are all no more than 0.06%. Therefore, the segregation of various elements in the zinc-aluminum-magnesium alloy ingot prepared in the embodiment of the present invention is effectively controlled.
[0126] It can be seen from Table 9 that compared with the smelting in the reverberatory furnace, the smelting and casting temperatures of the embodiment of the present invention are reduced by 80-100° C., the production cost is significantly reduced, the slag production rate in the alloy casting process is reduced by 15%, and the product remelting slag rate is reduced by 0.80%.
[0127] Table 8
[0128] batch 1 2 3 4 5 Al% 5.68 5.67 5.73 5.70 5.69 Mg% 1.89 1.88 1.91 1.87 1.88 Lanthanum-cerium mixed rare earth % 0.024 0.022 0.027 0.022 0.027 B% 0.0056 0.0058 0.0056 0.0062 0.0064 Ti% 0.030 0.032 0.025 0.033 0.031 Ca% 0.021 0.024 0.025 0.023 0.022 Si% 0.061 0.063 0.065 0.058 0.063 Sr% 0.028 0.032 0.026 0.028 0.031 Fe% 0.008 0.008 0.008 0.008 0.008 Pb% 0.0035 0.0036 0.0035 0.0037 0.0038 Cd% 0.002 0.0025 0.002 0.002 0.002 Cu% 0.002 0.002 0.002 0.002 0.002 Sn% <0.0005 <0.0005 <0.0005 <0.0005 <0.0005 V% - <0.002 <0.002 - -
[0129] Table 9
[0130]
[0131] The Fe content in the zinc-aluminum-magnesium alloy ingot prepared in the embodiment of the present invention is ≤0.008%, the oxide inclusions in the zinc-aluminum-magnesium alloy ingot are significantly reduced, the physical defects such as shrinkage cavities at the bottom of the alloy, internal shrinkage cavities, fish scales, cracks, etc. are significantly improved, and the product physical specification qualification rate reaches 96.3%.
[0132] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A zinc-aluminum-magnesium coating material, characterized in that: Calculated by mass percentage, it includes 5%-8% Al, 1.5%-3.0% Mg, 0.01%-0.06% lanthanum-cerium mixed rare earth, 0.05%-0.2% Si, 0.005%-0.02% B, 0.015%-0.1% Ti, 0.01%-0.06% Sr, 0.01%-0.08% Ca, and the balance is Zn and unavoidable impurities.
2. A method for preparing a zinc-aluminum-magnesium coating material, characterized in that: The steps include: Prepare metal raw materials according to the composition and content of claim 1: zinc ingot, aluminum ingot, magnesium ingot, aluminum-titanium-boron alloy, aluminum-silicon alloy, zinc-aluminum rare earth alloy, aluminum-calcium alloy and aluminum-strontium alloy; After the zinc ingot and the aluminum ingot are added into the core induction furnace for melting, aluminum-titanium-boron alloy, aluminum-silicon alloy, zinc-aluminum rare earth alloy, aluminum-calcium alloy and aluminum-strontium alloy are added at 520-560°C, and after smelting, the first part of the refining agent is added to slag, slag pounding and slag raking to obtain the zinc-aluminum molten liquid; Add magnesium ingots to the zinc-aluminum molten liquid in batches, and continue stirring for 20 to 40 minutes after smelting to obtain the zinc-aluminum-magnesium molten liquid; The second part of the refining agent is sprayed through the nitrogen adding pipe with nitrogen to the lower part of the zinc-aluminum-magnesium melt to form slag. After the refining agent is sprayed, nitrogen is continued to be introduced for 5 to 15 minutes, and then the slag is left to stand for 15 to 25 minutes, and the slag is pounded and raked, and the composition of the zinc-aluminum-magnesium alloy melt is tested; The zinc-aluminum-magnesium alloy melt is cast at one time, the temperature is 520-560℃, the mold temperature is not more than 70℃, and the surface slag is removed after casting; After casting is completed, when the cooling and solidification area of the casting blank is ≥90%, a cover plate is added or water is poured to form an alloy ingot; The mold and the surface of the alloy ingot are cooled by fan or / and water injection to forcefully cool the mold and the surface of the alloy ingot, so that the alloy ingot is completely solidified to obtain a zinc-aluminum-magnesium alloy ingot.
3. The method for preparing the zinc-aluminum-magnesium coating material according to claim 2, characterized in that: A spiral stirrer is arranged in the furnace body of the core induction furnace.
4. The method for preparing the zinc-aluminum-magnesium coating material according to claim 2, characterized in that: When the magnesium ingots are added to the zinc-aluminum melt in batches, each added magnesium ingot is pressed into the zinc-aluminum melt.
5. The method for preparing the zinc-aluminum-magnesium coating material according to claim 2, characterized in that: The total mass of the refining agent is 0.6% to 1% of the total mass of the metal raw material, the first part of the refining agent is 55 to 65% of the total mass of the refining agent, and the second part of the refining agent is 35 to 45% of the total mass of the refining agent.
6. The method for preparing the zinc-aluminum-magnesium coating material according to claim 5, characterized in that: The refining agent is a low-fluorine and low-chlorine refining agent comprising charcoal powder, silicon dioxide and river sand.
7. The method for preparing the zinc-aluminum-magnesium coating material according to claim 2, characterized in that: The cored induction furnace adopts a method of discharging the obtained zinc-aluminum-magnesium alloy melt from the bottom of the furnace body.
8. The method for preparing the zinc-aluminum-magnesium coating material according to claim 2, characterized in that: The zinc-aluminum-magnesium alloy melt enters the casting mold by blocking the chute with refractory bricks during one-time casting, and the chute is cleaned after casting.
9. The method for preparing the zinc-aluminum-magnesium coating material according to claim 2, characterized in that: When the casting blank is watered to form the initial alloy ingot, water is injected at the middle of the casting blank with a water column having a flow rate of less than 0.1 m / s to cool it, and water is sprayed at the edge of the mold to cool the mold temperature.
10. The method for preparing the zinc-aluminum-magnesium coating material according to claim 2, characterized in that: During the process of completely solidifying the alloy ingot to obtain the zinc-aluminum-magnesium alloy ingot, a small water column with a water flow rate of less than 0.1 m / s is used for water injection cooling or spray cooling, and the water is controlled to flow from the edge of the mold to the middle of the alloy ingot during water injection. Water is continuously injected for cooling at one time so that the water covers the alloy ingot, and the cooling time is 20-30 minutes.