Ta-Ti-Cu alloy with nanocrystalline structure and preparation method of Ta-Ti-Cu alloy

By preparing nanocrystalline Ta-Ti-Cu alloy, selective laser melting technology is used to form high-density, columnar crystal defect-free materials, which solves the problem of poor mechanical properties of tantalum alloys in SLM technology, and achieves high tensile strength and Materials with elongation, suitable for aerospace and medicine.

CN118957376AActive Publication Date: 2024-11-15INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411012749.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

When preparing tantalum alloys, the complex thermal history caused by its point-by-line deposition method, resulting in the microstructure of the material during the forming process is needle-shaped martensite α' that penetrates the primary columnar β grains. This leads to poor mechanical properties of materials, especially plasticity, limits their application in aerospace and medicine.

Method used

Using nanocrystalline structure Ta-Ti-Cu alloy, its chemical composition is Cu: 1-12%, Ti: 10-40%, and the balance is Ta. It is prepared by selective laser melting technology to form nano-size-grade thin strips of tissue and laser The power is 500-800W, the scanning speed is 1000-2500mm/s, the interlayer deflection angle is 30-90°, the energy density is 100-200J·mm-3, forming a material with a tensile strength ≥1200MPa and an elongation ≥12%.

Benefits of technology

A nanocrystal structure with high density and excellent mechanical properties without penetrating columnar crystal defects is achieved, the tensile strength and elongation are significantly improved, and excellent mechanical properties are maintained at 600°C and below, avoiding grain coarsening.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957376A_ABST
    Figure CN118957376A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of tantalum alloy materials, and provides a nanocrystalline structure Ta-Ti-Cu alloy and a preparation method of the nanocrystalline structure Ta-Ti-Cu alloy. 10 to 40 parts of Ti; and the balance being Ta. The preparation method of the alloy comprises the following steps: utilizing a selective laser melting technology, wherein the laser power is 500-800W, the scanning speed is 1000-2500mm. S <-1 >, the interlayer deflection angle is 30-90 degrees, and the energy density is 100-300J. Mm <-3 >. The microscopic structure of the prepared alloy is a nano-size-level thin strip structure, and the width of the thin strip structure ranges from 80 nm to 150 nm. The tensile strength of the Ta-Ti-Cu alloy with the nanocrystalline structure is larger than or equal to 1200 MPa, the ductility is larger than or equal to 12%, and the Ta-Ti-Cu alloy can be applied to the fields of aerospace, medical materials, industry and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of tantalum alloy materials, in particular to a nanocrystalline Ta-Ti-Cu alloy and a preparation method thereof. Background Art

[0002] Tantalum and tantalum alloys have been applied to many high-tech fields such as aerospace, metallurgy, chemical industry, and biomedicine due to their excellent chemical stability, high-temperature mechanical properties, corrosion resistance, processing and forming capabilities, and excellent bio-inertness and biocompatibility. Selective laser melting (SLM) is one of the fastest-growing and most widely used technologies in additive manufacturing (AM). Its characteristics are rapid melting and solidification of metal powders, and then rapid prototyping of metal parts with complex structures. The working principle of SLM technology is to use a preset laser scanning strategy to make the high laser beam melt the metal powder layer by layer according to the forming requirements of the part cross section to quickly form metal parts. SLM technology has the advantages of grain refinement, avoidance of segregation, energy saving and environmental protection, and one-time forming of complex structural parts. Therefore, the preparation of complex titanium alloy parts by SLM technology will have broad prospects in the fields of aerospace or medical equipment.

[0003] However, the point-by-point, line-by-line, and layer-by-layer deposition method of SLM technology produces a unique and complex thermal history composed of multiple non-steady-state horizontal and vertical thermal cycles, resulting in the microstructure of tantalum alloy in the forming process being composed of acicular martensite α' that penetrates the primary columnar β grains, resulting in poor mechanical properties of the material, especially plasticity, which greatly limits the application of SLM technology in the aerospace and medical fields. Summary of the invention

[0004] The purpose of the present invention is to provide a nanocrystalline Ta-Ti-Cu alloy and a preparation method thereof.

[0005] The nanocrystalline Ta-Ti-Cu alloy provided by the invention has the following chemical components by weight percentage: Cu: 1-12%, Ti: 10-40%, and the balance is Ta.

[0006] Furthermore, the weight percentage of Cu in the alloy is 3-9%.

[0007] The nanocrystalline Ta-Ti-Cu alloy provided by the present invention has a microstructure of nano-sized fine strips, and the width of the fine strips is 80-150nm. When the alloy is used for 2h at a temperature of less than or equal to 600°C, the grains do not coarsen and grow. The tensile strength of the alloy is ≥1200MPa, and the elongation is ≥12%.

[0008] The present invention provides a method for preparing a nanocrystalline Ta-Ti-Cu alloy, and the preparation method is as follows:

[0009] 1) Pre-setting Ta-Ti-Cu alloy powder to form a layer to be treated;

[0010] 2) performing selective laser melting on the layer to be processed according to printing process parameters to form a target layer;

[0011] 3) Repeat steps 1) to 2) to form a Ta-Ti-Cu alloy.

[0012] The invention provides a method for preparing a nanocrystalline Ta-Ti-Cu alloy. In the selective laser melting process, the laser power is 500-800W, the laser scanning speed is 1000-2500mm / s, the laser scanning spacing is 30-120μm, the interlayer deflection angle is 30-90°, and the energy density is 100-200J·mm -3 .

[0013] The nanocrystalline Ta-Ti-Cu alloy provided by the present invention is used in aerospace, medical equipment and industrial fields, and the medical equipment is oral and orthopedic implant medical equipment.

[0014] The beneficial effects of the present invention are:

[0015] (1) Different from the existing additive manufacturing method for preparing tantalum and its alloys (Ta-Ti, pure Ta), the nanocrystalline Ta-Ti-Cu alloy and its additive manufacturing method provided by the present invention do not have defects such as through-columnar defects, and the microstructure is a nano-sized fine strip structure. (Ti, as a solid solution of the Cu element, solves the problem of Ta-Cu immiscibility, improves the density of the additive manufacturing alloy, and makes the material free of Ta-Cu interface defects).

[0016] (2) The Ta-Ti-Cu alloy of the present invention has excellent mechanical properties and achieves strong-plastic matching. Its tensile strength is ≥1200 MPa and its elongation is ≥12%.

[0017] (3) The nanocrystalline Ta-Ti-Cu alloy provided by the present invention can maintain excellent mechanical properties when used at 600°C or below for 2 hours without coarsening or growing grains. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is a transmission electron microscope image of the alloy of Example 7;

[0019] Figure 2 is the transmission electron microscope image of the alloy of comparative example 2;

[0020] Figure 3This is the transmission electron microscope image of the alloy of comparative example 11. DETAILED DESCRIPTION

[0021] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.

[0022] Example:

[0023] A nanocrystalline Ta-Ti-Cu alloy, whose chemical composition is (by weight percentage): Cu: 1-12%; Ti: 10-40%; the balance is Ta. Examples 1-12 are Ta-Ti-Cu alloys prepared according to the chemical composition range provided by the present invention, and the content of Cu element is gradually increased, and the corresponding preparation process is also appropriately adjusted within the technical parameter range specified by the present invention. Examples 3-8 are preferred Cu content ranges of the present invention. See Table 1 for details.

[0024] Table 1 Chemical composition and preparation process of the examples

[0025]

[0026] Comparative Example:

[0027] The chemical composition of Comparative Examples 1-2 is lower than the lower limit of the chemical composition range provided by the present invention, and the chemical composition of Comparative Examples 11-12 is higher than the upper limit of the chemical composition range provided by the present invention. The laser power of Comparative Example 3 is lower than the lower limit of the laser power range provided by the present invention; the laser power of Comparative Example 4 is higher than the upper limit of the range provided by the present invention; the scanning speed of Comparative Example 5 is lower than the lower limit of the range provided by the present invention; the scanning speed of Comparative Example 6 is higher than the upper limit of the range provided by the present invention; the interlayer deflection angle of Comparative Example 7 is lower than the lower limit of the range provided by the present invention; the interlayer deflection angle of Comparative Example 8 is higher than the upper limit of the range provided by the present invention; the energy density of Comparative Examples 9 and 10 is lower or higher than the lower limit or upper limit of the range provided by the present invention, respectively. See Table 2 for details.

[0028] Table 2 Chemical composition and preparation process of comparative examples

[0029]

[0030] 1. Tensile performance test

[0031] The room temperature tensile mechanical properties of the comparative example and the example materials were tested using an Instron 8872 tensile testing machine, with a tensile rate of 0.5 mm / min. Before the test, the material was processed into a standard tensile specimen with a thread diameter of 10 mm, a gauge diameter of 5 mm, and a gauge length of 30 mm using a lathe. Three parallel samples were taken from each group of heat-treated (additive manufacturing material) specimens. The mechanical properties obtained from the experiment include tensile strength and elongation. The specific results are shown in Table 3.

[0032] 2. Grain size statistics

[0033] The electron backscatter diffraction (EBSD) analysis system of the scanning electron microscope was used to perform phase volume fraction (organization size) statistics on the samples before and after fatigue. The sample preparation method was to first mechanically polish the sample to obtain a smooth surface, and then place the sample in an electrolyte (6% perchloric acid + 30% butanol + 64% methanol) at -25°C for electrolytic polishing for 20 seconds to remove surface stress. When EBSD data was collected, the scanning electron microscope had an operating voltage of 20kV, a current of 18nA, a step size of 0.2μm, and a scanning range resolution of more than 80%. The grain size was analyzed using Channel 5 software. The specific results are shown in Tables 3 and 4.

[0034] Table 3 Mechanical properties and organizational dimensions of the examples and comparative examples

[0035]

[0036]

[0037] Table 4 Organization characteristics of the materials of the embodiments and comparative examples and organizational changes after being kept at different temperatures for 2 hours

[0038]

[0039] The transmission electron microscope images of the alloys of Example 7, Comparative Example 2 and Comparative Example 11 are as follows: Figure 1-Figure 3 . From the results in Tables 3 and 4, it can be seen that Examples 1 to 12 are all nano-lath structures, and have high strength and good plasticity. However, since the Cu content range of Comparative Examples 1, 2, 11, and 12 is not within the range required by the present invention, their mechanical properties are ultimately poor, or their structures are coarse lath structures. Since the process parameter ranges of Comparative Examples 3-10 are not within the range required by the present invention, such as laser power and scanning speed, the mechanical properties of the prepared materials are poor, and no nanocrystalline lath structure is obtained.

[0040] From the results in Table 4, it can be seen that Examples 3-8 have good thermal stability of the structure during aging at 600°C or below, and the lath size does not change significantly after aging. Since the original lath size of Examples 1, 2, 9-12 is larger than that of Examples 3-8, the lath size grows to the range of 300-500nm during aging at 600°C or below, and the thermal stability of the structure is slightly worse than that of Examples 3-8 of the present invention, but is better than that of Comparative Example 1. From Table 4, it can be seen that the lath of Comparative Example 1 undergoes significant coarsening and growth.

[0041] Although the present invention has been disclosed as above in some embodiments, it is not intended to limit the present invention. Any technical personnel in this field can make possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the main purpose and scope of the present invention. Therefore, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the protection scope of the technical solution of the present invention.

Claims

1. A nanocrystalline Ta-Ti-Cu alloy, characterized in that: The chemical composition of the alloy is as follows by weight: Cu: 1-12%, Ti: 10-40%, and the balance is Ta.

2. The nanocrystalline Ta-Ti-Cu alloy according to claim 1, characterized in that: The weight percentage of Cu in the alloy is 3-9%.

3. The nanocrystalline Ta-Ti-Cu alloy according to claim 1 or 2, characterized in that: The microstructure of the alloy is a nanometer-sized fine strip structure, and the width of the fine strip structure is 80 to 150 nm.

4. The nanocrystalline Ta-Ti-Cu alloy according to claim 1 or 2, characterized in that: When the alloy is used for 2 hours at a temperature less than or equal to 600°C, the grains do not coarsen and grow.

5. The nanocrystalline Ta-Ti-Cu alloy according to claim 1 or 2, characterized in that: The tensile strength of the alloy is ≥1200MPa and the elongation is ≥12%.

6. A method for preparing a nanocrystalline Ta-Ti-Cu alloy according to claim 1 or 2, characterized in that: The preparation method is as follows: 1) Pre-setting Ta-Ti-Cu alloy powder to form a layer to be treated; 2) performing selective laser melting on the layer to be processed according to printing process parameters to form a target layer; 3) Repeat steps 1) to 2) to form a Ta-Ti-Cu alloy.

7. The method for preparing a nanocrystalline Ta-Ti-Cu alloy according to claim 6, characterized in that: In the selective laser melting process, the laser power is 500-800W, the laser scanning speed is 1000-2500mm / s, the laser scanning spacing is 30-120μm, the interlayer deflection angle is 30-90°, and the energy density is 100-200J·mm -3 .

8. Application of the nanocrystalline Ta-Ti-Cu alloy according to claim 1 or 2 in aerospace, medical equipment and industrial fields.

9. The use according to claim 8, characterized in that: The medical device is an oral or orthopedic implant medical device.

Citation Information

Patent Citations

  • Nanocrystalline structure Ti-Cu alloy and selective laser melting additive manufacturing preparation method thereof

    CN112251642A

  • Ultralow elastic modulus antibacterial medical tantalum alloy and preparation method thereof

    CN114540689A

  • Composition of orthopedic knee implant and the method for manufacture thereof

    US20170071744A1

  • Metallic glassy alloy powders for antibacterial coating

    US9609874B1