Method for improving hardness uniformity of steel rail tread

Through rare earth element treatment and fine smelting technology, the contact fatigue problem caused by unevenness of the rail tread hardness is solved, and the uniformity of the rail hardness and service life are improved, thereby reducing maintenance costs.

CN118957392APending Publication Date: 2024-11-15BAOTOU IRON & STEEL (GROUP) CO LTD

Patent Information

Application Number
CN202410935629.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During service, contact fatigue damage and wear problems caused by uneven tread hardness of the rails, resulting in shortening of the service life of the line.

Method used

Rare earth element treatment technology is adopted, combined with converter smelting, LF refining, VD vacuum degassing and continuous casting technology, to control the chemical composition and structure of the rails, ensure the uniformity of the tread hardness in the length direction, and through specific rolling processes and heat treatment Method to reduce hardness fluctuations.

Benefits of technology

It significantly improves the uniformity of the rail tread hardness, reduces uneven wear, extends the service life of the rail, and reduces the line maintenance cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004941236840000031
    Figure BDA0004941236840000031
  • Figure BDA0004941236840000041
    Figure BDA0004941236840000041
Patent Text Reader

Abstract

The invention discloses a method for improving steel rail tread hardness uniformity. The production process comprises the steps of molten iron pretreatment, converter smelting, LF ladle refining, VD vacuum degassing, continuous casting, steel billet heating and steel rail rolling. The steel rail rolling technology comprises the steps of square billet continuous casting, saw cutting, heating, BD1 rolling, BD2 rolling, CCS universal rolling mill continuous rolling, heat treatment, cooling bed cooling, straightening, flaw detection, checking, machining and warehousing. The steel rail comprises the following chemical components in percentage by weight: 0.71-0.80% of C; s : 0.50 to 0.80%; mn: 0.75 to 1.05%; less than or equal to 0.020% of Ce; less than or equal to 0.025% of P; s is less than or equal to 0.025%; al < = 0.010%; and the balance of Fe and inevitable impurities. According to the method, the hardness value fluctuation of the tread center line of the same steel rail in the length direction is smaller than 5 HBW, and the serious uneven abrasion phenomenon caused by too large hardness fluctuation of the tread of the steel rail is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgical engineering, and in particular relates to a method for improving the hardness uniformity of a rail tread. Background Art

[0002] With the increase in railway operating mileage and the trend towards high speed and heavy load, the phenomenon of contact fatigue damage of rails during service is becoming more and more frequent. Tread hardness is a key performance indicator of rails. High and uniform tread hardness ensures good and stable wear resistance of rails, preventing premature fatigue damage or excessive wear in some areas of the rails, which shortens the service life of the line. Taking U75VH rails as an example, it has the advantages of high strength, toughness and fatigue resistance, and is still widely used in my country's railway lines. For U75VH rails, the hardness requirement of the rail head tread is 340-400HBW, and the hardness deviation range on the center line of the tread of the same rail is required to be no more than 30HBW. If the deviation range of the hardness of the rail tread is too large, it will cause serious uneven wear of the rail, deteriorate the wheel-rail contact state, aggravate the complexity of the stress distribution of the wheel-rail contact surface, lead to the generation of fatigue cracks, and further lead to the peeling and falling of the rail tread. Summary of the invention

[0003] The purpose of the present invention is to provide a method for improving the uniformity of the hardness of the rail tread. By adding rare earth elements, a rail with good strength and toughness matching is smelted and rolled, and the hardness value fluctuation of the tread center line of the same rail in the length direction is made less than 5HBW, effectively avoiding serious uneven wear caused by excessive fluctuation of the rail tread hardness, and improving the service life of the rail.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] The present invention provides a method for improving the uniformity of hardness of a rail tread, comprising:

[0006] Production process: hot metal pretreatment - converter smelting - LF ladle refining - VD vacuum degassing - continuous casting - billet heating - rail rolling;

[0007] The converter smelting adopts aluminum-free deoxidation alloying, and the whole process is argon-blown as normal refining; vacuum degree ≤ 0.10KPa, deep vacuum time ≥ 18min, superheat ΔT ≤ 30℃, and rare earth wire is added at the VD station;

[0008] The rail rolling process is: continuous casting billet - sawing - heating - BD1 rolling - BD2 rolling - CCS universal rolling mill continuous rolling - heat treatment - cooling on cooling bed - straightening - flaw detection - inspection - processing - storage; the temperature of the billet heating and preheating section is not more than 800℃; the heating temperature is 1200℃, and the heating time is not less than 3 hours; the furnace temperature is not less than 1100℃, the rolling temperature is 1080℃~1150℃, and the final rolling temperature is 900~950℃; the starting cooling temperature of the online heat-treated rail is 750℃~850℃, the temperature of the heat treatment line is 520~560℃, the total time of online heat treatment is 120~160s, and the cooling rate is 1.0℃ / s~3.0℃ / s;

[0009] The chemical composition of the rail includes by weight: C: 0.71-0.80%; Si: 0.50-0.80%; Mn: 0.75-1.05%; Ce≤0.020%; P≤0.025%; S≤0.025%; Al≤0.010%; the remainder is Fe and unavoidable impurities.

[0010] Furthermore, the chemical composition of the rail includes by weight: C: 0.79%; Si: 0.66%; Mn: 0.94%; V: 0.073%; Ce: 0.0007%; P: 0.014%; S: 0.003%; Al: 0.003%; the remainder is Fe and unavoidable impurities.

[0011] Furthermore, the chemical composition of the rail includes by weight: C: 0.78%; Si: 0.64%; Mn: 0.95%; V: 0.073%; Ce: 0.0004%; P: 0.014%; S: 0.005%; Al: 0.002%; the remainder is Fe and unavoidable impurities.

[0012] Furthermore, the chemical composition of the rail includes by weight: C: 0.80%; Si: 0.66%; Mn: 0.96%; V: 0.074%; Ce: 0.0008%; P: 0.013%; S: 0.004%; Al: 0.004%; the remainder is Fe and unavoidable impurities.

[0013] Furthermore, the rail structure is pearlite, a small amount of ferrite is allowed, and the decarburization layer is ≤0.5mm.

[0014] Furthermore, the tensile strength is ≥1180 MPa and the elongation is ≥10%.

[0015] Compared with the prior art, the beneficial technical effects of the present invention are:

[0016] Rail structure is pearlite, with a small amount of ferrite allowed, decarburization layer ≤ 0.5mm, tensile strength ≥ 1180MPa, elongation ≥ 10%.

[0017] Under the premise of meeting the standard composition, performance requirements and existing process routes, the present invention adopts a rare earth treatment process to purify the steel and make the structure transformation uniform. While ensuring that various properties of the rails meet the standard requirements, the hardness uniformity of the rail tread is improved, the maintenance cost of the line rails is reduced, and the service safety performance and service life of the rails are improved. DETAILED DESCRIPTION

[0018] A method for improving the uniformity of the hardness of a rail tread, wherein the smelting production process of the rail is: molten iron → converter smelting → LF refining → VD → continuous casting. The converter smelting adopts aluminum-free deoxidation alloying, and the whole process is argon-blown as normal refining; the vacuum degree is ≤0.10KPa, the deep vacuum time is ≥18min, the superheat ΔT is ≤30°C, and the rare earth wire is added at the VD station.

[0019] The smelting chemical composition control of Examples 1-3 of the present invention and Comparative Examples 1-3 is shown in Table 1. Examples 1-3 are respectively carried out according to the composition range of Comparative Examples 1-3, and rare earth treatment is added. The chemical composition of each embodiment is shown in Table 1.

[0020] Table 1 Comparison of different components during implementation (wt.%)

[0021]

[0022]

[0023] The rail rolling process is: continuous casting billet - sawing - heating - BD1 rolling - BD2 rolling - CCS universal rolling mill continuous rolling - heat treatment - cooling on cooling bed - straightening - flaw detection - inspection - processing - storage. The temperature of the billet heating preheating section is not more than 800℃; the heating temperature is 1200℃, and the heating time is not less than 3 hours; the furnace temperature is not less than 1100℃, the rolling temperature is 1080℃~1150℃, and the final rolling temperature is 900~950℃; the cooling temperature of the online heat treatment rail is 750℃~850℃, the temperature of the heat treatment line is 520~560℃, the total time of online heat treatment is 120~160s, and the cooling rate is 1.0℃ / s~3.0℃ / s.

[0024] The tread hardness is randomly sampled on the rail, the sample length is 250mm, the top surface of the rail head is ground off 0.5mm, and 5 points are tested for Brinell hardness test. The average value, variance and standard deviation are calculated. The test temperature is 20℃±5℃. The above sample sampling method, position and size are in accordance with TB / T 2344.1-2020 standard. The test results of the centerline hardness of the rail tread of the embodiment and comparative example are shown in Table 2.

[0025] Table 2 Hardness test results (HBW) of various embodiments of the present invention and comparative examples

[0026] project 1 2 3 4 5 Example 1 362 361 361 361 361 Example 2 361 362 363 363 363 Example 3 359 360 359 359 359 Comparative Example 1 362 365 361 366 370 Comparative Example 2 371 364 362 364 365 Comparative Example 3 370 360 363 366 365

[0027] The uniformity of the centerline hardness values ​​of the rail treads of the embodiments and comparative examples is shown in Table 3.

[0028] Table 3 Comparison of the uniformity of the centerline hardness values ​​of the rail treads of the embodiment and the comparative example (HBW)

[0029] project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Minimum 362 361 359 361 362 360 Maximum 361 363 360 370 371 370 Biggest changes 1 2 1 9 9 10 average value 361.2 362.4 359.2 364.8 365.2 364.8 variance 0.2 0.8 0.2 12.7 11.7 13.7 Standard Deviation 0.45 0.89 0.45 3.56 3.42 3.70

[0030] It can be seen that the hardness fluctuation of the center line of the heat-treated rail tread produced by the method of the present invention does not exceed 5HBW (actually within 2HBW), the hardness value fluctuation range is reduced by more than 60%, the hardness uniformity of the center line of the rail tread is greatly improved, and the control effect is good.

[0031] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for improving the uniformity of rail tread hardness, characterized in that: include: Production process: hot metal pretreatment - converter smelting - LF ladle refining - VD vacuum degassing - continuous casting - billet heating - rail rolling; The converter smelting adopts aluminum-free deoxidation alloying, and the whole process is argon-blown as normal refining; vacuum degree ≤ 0.10KPa, deep vacuum time ≥ 18min, superheat ΔT ≤ 30℃, and rare earth wire is added at the VD station; Rail rolling process: continuous casting billet - sawing - heating - BD1 rolling - BD2 rolling - CCS universal rolling mill continuous rolling - heat treatment - cooling on cooling bed - straightening - flaw detection - inspection - processing - storage; the temperature of the billet heating and preheating section is not more than 800℃; the heating temperature is 1200℃, and the heating time is not less than 3 hours; the furnace temperature is not less than 1100℃, the rolling temperature is 1080℃~1150℃, and the final rolling temperature is 900~950℃; the cooling temperature of the online heat-treated rail is 750℃~850℃, the temperature of the heat treatment line is 520~560℃, the total time of online heat treatment is 120~160s, and the cooling rate is 1.0℃ / s~3.0℃ / s; The chemical composition of the rail includes by weight: C: 0.71~0.80%; Si: 0.50~0.80%; Mn: 0.75~1.05%; Ce≤0.020%; P≤0.025%; S≤0.025%; Al≤0.010%; the balance is Fe and unavoidable impurities.

2. The method for improving the uniformity of rail tread hardness according to claim 1, characterized in that: The chemical composition of the rail includes by weight: C: 0.79%; Si: 0.66%; Mn: 0.94%; V: 0.073%; Ce: 0.0007%; P: 0.014%; S: 0.003%; Al: 0.003%; the remainder is Fe and unavoidable impurities.

3. The method for improving the uniformity of rail tread hardness according to claim 1, characterized in that: The chemical composition of the rail includes by weight: C: 0.78%; Si: 0.64%; Mn: 0.95%; V: 0.073%; Ce: 0.0004%; P: 0.014%; S: 0.005%; Al: 0.002%; the remainder is Fe and unavoidable impurities.

4. The method for improving the uniformity of rail tread hardness according to claim 1, characterized in that: The chemical composition of the rail includes by weight: C: 0.80%; Si: 0.66%; Mn: 0.96%; V: 0.074%; Ce: 0.0008%; P: 0.013%; S: 0.004%; Al: 0.004%; the remainder is Fe and unavoidable impurities.

5. The method for improving the uniformity of rail tread hardness according to claim 1, characterized in that: The rail structure is pearlite, a small amount of ferrite is allowed, and the decarburization layer is ≤0.5mm.

6. The method for improving the uniformity of rail tread hardness according to claim 1, characterized in that: Tensile strength ≥1180MPa, elongation ≥10%.

Citation Information

Patent Citations

  • Production method for improving hardness uniformity of tread of heat-treated steel rail and obtained steel rail

    CN114058824A

  • Manufacturing method for improving low-temperature toughness of hot-rolled U75V steel rail through rare earth elements

    CN114855082A

  • Production method for improving wear resistance of steel rail

    CN115896599A

  • Production method of heavy haul railway large-radius curve heat treatment steel rail

    CN115971239A

  • Production method of U76CrRE steel rail

    CN117210742A

Cited By

  • Manufacturing method for improving yield strength of exit steel rail through rare earth

    CN119843142A