Control method for non-metallic inclusions of steel rail steel
By controlling the binary alkalinity and argon flow rate of refining slag in the ladle during the smelting process of rail steel, combined with vacuum treatment and alloying, the sulfur content and sulfide inclusion rating in the rail steel was successfully reduced, and the existing technology was solved The problem of controlling non-metallic inclusions improves the fatigue life and welding performance of steel.
Patent Information
- Application Number
- CN202411031008.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art control of non-metallic inclusions in rail steel is difficult to effectively reduce sulfide inclusion rating and improve fatigue life. The commonly used high-alkali refined slag treatment method will lead to an increase in brittle inclusion content in steel, affecting welding performance and use. life.
Using a lower binary alkalinity of the refining slag in ladle, the liquid steel temperature and argon flow are controlled during the smelting of the converter and LF furnace, combined with vacuum treatment and alloying, to ensure that the brittle inclusions are converted into plastic inclusions, and through large argon The flow rate is strongly stirred to effectively remove sulfide inclusions.
The sulfur content in rail steel is reduced, ensuring that the sulfide inclusion rating is less than or equal to 2.5, improving the fatigue resistance and service life of the steel, while avoiding the increase in brittle inclusion and improving welding performance.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel smelting, and in particular relates to a method for controlling non-metallic inclusions in rail steel. Background Art
[0002] Rails are one of the important components of railways. During railway transportation, they come into contact with wheels made of the same steel material, provide effective support and guidance for locomotives, and must withstand huge vertical pressure and strong lateral friction from the wheels. Modern railway transportation is developing at a rapid pace, especially as my country's railway transportation continues to move towards high speed and heavy loads. The transportation load is increasing year by year, which puts more stringent requirements on the quality of rails. When the rails come into contact with the wheels, they bear the reciprocating and variable loads of the locomotives. The non-metallic inclusions they contain have an important impact on the fatigue life of the rails. Sulfide inclusions represented by manganese sulfide are generally precipitated by combining elements such as Mn and Fe with S during the solidification process of the ingot. They have the characteristics of low melting points, so they gather in specific areas such as grain boundaries, dendrites and central areas of the ingot, causing damage such as looseness, shrinkage, and segregation; sulfide inclusions can make steel hot and brittle, and at the same time, the gathered sulfide inclusions are stretched and elongated during the rolling process of the rail, cutting the steel matrix and reducing the transverse mechanical properties, such as affecting the low-temperature transverse impact toughness of the steel. Oxide inclusions are generally brittle inclusions, which will destroy the continuity of the steel matrix in steel, easily cause stress concentration, and can significantly reduce the plasticity, impact toughness, corrosion resistance, wear resistance, fatigue resistance and toughness of the weld metal of the steel, and affect the processing performance of the material; silicate inclusions have the characteristics of low melting points, and they are difficult to float and remove during the smelting process, so they are easy to gather and grow during the solidification process of the ingot, and are stretched and elongated during the rolling process of the rail, cutting the steel matrix, affecting the service life of the steel. Both spherical oxide inclusions and single-particle spherical inclusions are not easy to deform, which causes local stress concentration in the steel, resulting in cracks and fractures, which greatly affects the fatigue resistance of the steel.
[0003] Due to the obstruction of non-metallic inclusions on the continuity of steel matrix structure, the steel is separated from non-metallic inclusions during rolling, heat treatment, welding and use, resulting in defects such as holes and cracks, which have a negative impact on the mechanical properties, corrosion resistance, fatigue resistance, weldability and other indicators of steel. In particular, for the production of rails, a series of influencing factors such as large deformation rolling, complex heat treatment process, special stress conditions and climate environment have a more direct adverse effect on service life. The control of non-metallic inclusions in rail steel has always been the object of research for metallurgical workers.
[0004] In order to control non-metallic inclusions in the production process of domestic rail steel, some adopt high-basicity refined slag system, some add a certain amount of Al2O3 to the refined slag, and some use elements such as calcium and rare earth to modify the steel to remove non-metallic inclusions. However, these methods have great negative effects. The content of brittle inclusions in steel increases, which is not conducive to improving the fatigue life of rails and affects their welding performance and service use. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a method for controlling non-metallic inclusions in rail steel. The method adopts a lower binary basicity of the refined slag in the ladle to ensure the transformation of brittle inclusions in the steel into plastic inclusions, while avoiding the problems of poor desulfurization effect of molten steel caused by the lower binary basicity of the refined slag in the ladle and high sulfur content in the finished rails resulting in high sulfide inclusion rating of the rails.
[0006] The present invention provides a method for controlling non-metallic inclusions in rail steel, comprising the following steps:
[0007] A) Converter smelting:
[0008] Adding molten iron with a sulfur content of ≤0.02wt% into the converter to carry out converter smelting, and controlling the carbon content of the molten steel at the end of the smelting to be 0.03-0.15wt%; adding alloys and carburizers required for the steel grade into the ladle during the steel tapping process after the converter smelting, and adding active lime when the steel tapping reaches 30-40%;
[0009] B) LF furnace refining:
[0010] After completing the treatment of step A), the ladle is sent to the LF furnace for refining, and siliceous refining slag, active lime and fluorite are added to the ladle in turn, and the flow rate of argon blowing is adjusted to 1.5-2.5NL / min per ton of steel, and the molten steel is heated and refined. When the molten steel temperature is the target temperature + 20-30°C, the flow rate of argon blowing is adjusted to 4-5NL / min per ton of steel. At this flow rate, argon is blown at the bottom for 5-10 minutes. At this time, the binary basicity of the refined slag in the ladle is 1.6-2.4. When the molten steel temperature meets the target requirements, argon blowing is stopped and the molten steel is discharged;
[0011] C) RH vacuum treatment:
[0012] After the molten steel treated in step B) enters the station, the molten steel is subjected to RH vacuum treatment; during the entire process of vacuum treatment, the lifting gas flow rate is controlled to be 9-13NL / min per ton of steel, and the vacuum degree is ≤100Pa; after vacuum treatment for 15-19min, the vacuum degree is maintained, and then alloy is added for alloying treatment; after alloying, the vacuum treatment is continued for more than 5min to make the composition uniform, and the vacuum is broken; then, the bottom argon blowing is carried out for more than 3min under the condition of adjusting the blowing argon flow rate to 0.5-0.8NL / min per ton of steel, and the molten steel exits the station;
[0013] D) Continuous casting and rolling:
[0014] The molten steel treated in step C) is continuously cast, and then the obtained continuously cast billet is rolled to obtain rail steel.
[0015] Preferably, in step A), active lime is added when the steel tapping reaches 35%.
[0016] Preferably, in step A), the amount of active lime added is 1.5-3.5 kg per ton of molten steel.
[0017] Preferably, in step A), the CaO content of the active lime is ≥ 85 wt%.
[0018] Preferably, in step B), the amount of the siliceous refined slag added is 1.5-6 kg per ton of molten steel.
[0019] Preferably, in step B), the SiO2 content of the siliceous refined slag is 30-50wt%, and the CaO content is 30-45wt%.
[0020] Preferably, in step B), the amount of active lime added is 2.5-4.5 kg per ton of molten steel.
[0021] Preferably, in step B), the CaO content of the active lime is ≥ 85 wt%.
[0022] Preferably, in step B), the amount of fluorite added is 15-25wt% of the amount of active lime added.
[0023] Preferably, in step B), the CaF2 content of the fluorite is ≥ 75wt%.
[0024] Compared with the prior art, the present invention provides a method for controlling non-metallic inclusions in rail steel, comprising the following steps: A) converter smelting: adding molten iron with an S content of ≤0.02wt% into the converter, performing converter smelting, and controlling the carbon content of the molten steel at the end of smelting to be 0.03-0.15wt%; after the converter smelting is completed, adding alloys and carburizers required for the steel grade into the ladle during the steel tapping process, and adding active lime when the steel tapping reaches 30-40%; B) LF furnace refining: after completing the treatment of step A), sending the ladle to the LF furnace for refining, adding siliceous refining slag, active lime and fluorite into the ladle in turn, adjusting the flow rate of argon blowing to 1.5-2.5NL / min per ton of steel, performing steel liquid heating and refining, and when the temperature of the molten steel is the target temperature + 20-30°C, adjusting the flow rate of argon blowing to 4-5NL / min per ton of steel, and bottom blowing argon at this flow rate Argon is blown for 5 to 10 minutes, at which time the binary basicity of the refined slag in the ladle is 1.6 to 2.4. When the temperature of the molten steel meets the target requirement, argon blowing is stopped and the molten steel leaves the station; C) RH vacuum treatment: after the molten steel treated in step B) enters the station, the molten steel is subjected to RH vacuum treatment; during the entire process of vacuum treatment, the lifting gas flow rate is controlled to be 9 to 13 NL / min per ton of steel, and the vacuum degree is ≤100 Pa; after vacuum treatment for 15 to 19 minutes, the vacuum degree is maintained, and then alloy is added for alloying treatment; after alloying, the vacuum treatment is continued for more than 5 minutes to make the composition uniform and the vacuum is broken; then, the bottom argon blowing is carried out for more than 3 minutes under the condition of adjusting the argon blowing flow rate to 0.5 to 0.8 NL / min per ton of steel, and the molten steel leaves the station; D) continuous casting and rolling: the molten steel treated in step C) is continuously cast, and then the obtained continuous casting billet is rolled to obtain rail steel. The invention adopts a relatively low binary basicity of the refining slag in the ladle during the LF refining process, makes the molten steel reach a relatively high temperature at the end of the LF refining, and simultaneously adopts a large argon gas flow rate to strongly stir the molten steel and the refining slag in the ladle, effectively removes sulfur in the steel while ensuring that the brittle inclusions in the steel are transformed into plastic inclusions, and reduces the temperature of the molten steel to a target range at the end of the LF refining furnace, ensures that the ratings of B and D class inclusions in the steel are both ≤1.0, the rating of Ds class inclusions is ≤0.5, the rating of A class inclusions is ≤2.5, and the rating of C class inclusions is ≤1.5 (A class inclusions refer to sulfide inclusions, B class inclusions refer to oxide inclusions, C class inclusions refer to silicate inclusions, D class inclusions refer to spherical oxide inclusions, and Ds class inclusions refer to single-particle spherical inclusions), and is suitable for producing high-quality rail steel. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] The present invention provides a method for controlling non-metallic inclusions in rail steel, comprising the following steps:
[0027] A) Converter smelting:
[0028] Adding molten iron with a mass content of S ≤ 0.020wt% into the converter, performing converter smelting, and controlling the carbon content of the molten steel at the end of smelting to be 0.03-0.15wt%; adding alloys and carburizers required for the steel grade into the ladle during the steel tapping process after the converter smelting, and adding active lime when the steel tapping reaches 35%;
[0029] B) LF furnace refining (LF: ladle furnace- ladle furnace):
[0030] After completing the treatment of step A), the ladle is sent to the LF furnace for refining, and siliceous refining slag, active lime and fluorite are added to the ladle in turn, and the flow rate of argon blowing is adjusted to 1.5-2.5 NL / min per ton of steel, and the molten steel is heated and refined. When the molten steel temperature is the target temperature + 20-30°C, the flow rate of argon blowing is adjusted to 4.0-5.0 NL / min per ton of steel. At this flow rate, argon is blown at the bottom for 5-10 minutes. At this time, the binary basicity of the refined slag in the ladle is 1.6-2.4. When the molten steel temperature meets the target requirements, argon blowing is stopped, and the molten steel is discharged;
[0031] C) RH vacuum treatment (RH: Ruhstahlhausenprocess, a vacuum degassing method commonly used in steelmaking):
[0032] After the molten steel treated in step B) enters the station, the molten steel is subjected to RH vacuum treatment; during the entire process of vacuum treatment, the lifting gas flow rate is controlled to be 9-13NL / min per ton of steel, and the vacuum degree is ≤100Pa; after vacuum treatment for 15-19min, the vacuum degree is maintained, and then alloy is added for alloying treatment; after alloying, the vacuum treatment is continued for more than 5min to make the composition uniform, and the vacuum is broken; then, the bottom argon blowing is carried out for more than 3min under the condition of adjusting the blowing argon flow rate to 0.5-0.8NL / min per ton of steel, and the molten steel exits the station;
[0033] D) Continuous casting and rolling:
[0034] The molten steel treated in step C) is continuously cast, and then the obtained continuously cast billet is rolled to obtain rail steel.
[0035] In the method provided by the present invention, in step A), the S content of the molten iron may specifically be 0.001wt%, 0.002wt%, 0.003wt%, 0.004wt%, 0.005wt%, 0.006wt%, 0.007wt%, 0.008wt%, 0.009wt%, 0.01wt%, 0.011wt%, 0.012wt%, 0.013wt%, 0.014wt%, 0.015wt%, 0.016wt%, 0.017wt%, 0.018wt%, 0.019wt% or 0.02wt%.
[0036] In the method provided by the present invention, in step A), the smelting temperature of the converter smelting is preferably 1630-1660°C, specifically 1630°C, 1635°C, 1640°C, 1645°C, 1650°C, 1655°C or 1660°C.
[0037] In the method provided by the present invention, in step A), the carbon content of the molten steel at the end point of the smelting can be specifically controlled at 0.03wt%, 0.04wt%, 0.05wt%, 0.06wt%, 0.07wt%, 0.08wt%, 0.09wt%, 0.1wt%, 0.11wt%, 0.12wt%, 0.13wt%, 0.14wt% or 0.15wt%.
[0038] In the method provided by the present invention, in step A), the S content of the molten steel at the end point of smelting is preferably ≤0.02wt%, specifically 0.001wt%, 0.002wt%, 0.003wt%, 0.004wt%, 0.005wt%, 0.006wt%, 0.007wt%, 0.008wt%, 0.009wt%, 0.01wt%, 0.011wt%, 0.012wt%, 0.013wt%, 0.014wt%, 0.015wt%, 0.016wt%, 0.017wt%, 0.018wt%, 0.019wt% or 0.02wt%.
[0039] In the method provided by the present invention, in step A), the alloy includes but is not limited to ferrosilicon, ferromanganese and the like.
[0040] In the method provided by the present invention, in step A), adding active lime when the steel tapping reaches 30-40% means that after 30-40% of the molten steel in the steel converter enters the ladle, active lime is added to the ladle. More specifically, active lime is added when the steel tapping reaches 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39% or 40%.
[0041] In the method provided by the present invention, in step A), the CaO content of the active lime is preferably ≥85wt%; the amount of active lime added is preferably 1.5-3.5kg per ton of molten steel, specifically 1.5kg, 1.6kg, 1.7kg, 1.8kg, 1.9kg, 2kg, 2.1kg, 2.2kg, 2.3kg, 2.4kg, 2.5kg, 2.6kg, 2.7kg, 2.8kg, 2.9kg, 3kg, 3.1kg, 3.2kg, 3.3kg, 3.4kg or 3.5kg.
[0042] In the method provided by the present invention, in step B), the siliceous refining slag contains SiO2, and its SiO2 content is preferably 30-50wt%, specifically 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt%, 40wt%, 41wt%, 42wt%, 43wt%, 44wt%, 45wt%, 46wt%, 47wt%, 48wt%, 49wt% or 50wt%; the CaO content of the siliceous refining slag is preferably 30-45wt%, specifically 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt%, 40wt%, 41wt%, 42wt%, 43wt%, 44wt% or 45wt%.
[0043] In the method provided by the present invention, in step B), the amount of the siliceous refined slag added is preferably 1.5-6 kg per ton of molten steel, specifically 1.5 kg, 1.6 kg, 1.7 kg, 1.8 kg, 1.9 kg, 2 kg, 2.1 kg, 2.2 kg, 2.3 kg, 2.4 kg, 2.5 kg, 2.6 kg, 2.7 kg, 2.8 kg, 2.9 kg, 3 kg, 3.1 kg, 3.2 kg, 3.3 kg g, 3.4kg, 3.5kg, 3.6kg, 3.7kg, 3.8kg, 3.9kg, 4kg, 4.1kg, 4.2kg, 4.3kg, 4.4kg, 4.5kg, 4.6kg, 4 .7kg, 4.8kg, 4.9kg, 5kg, 5.1kg, 5.2kg, 5.3kg, 5.4kg, 5.5kg, 5.6kg, 5.7kg, 5.8kg, 5.9kg or 6kg.
[0044] In the method provided by the present invention, in step B), the CaO content of the active lime is preferably ≥85wt%; the amount of active lime added is preferably 2.5-4.5kg per ton of molten steel, specifically 2.5kg, 2.6kg, 2.7kg, 2.8kg, 2.9kg, 3kg, 3.1kg, 3.2kg, 3.3kg, 3.4kg, 3.5kg, 3.6kg, 3.7kg, 3.8kg, 3.9kg, 4kg, 4.1kg, 4.2kg, 4.3kg, 4.4kg or 4.5kg.
[0045] In the method provided by the present invention, in step B), the CaF2 content of the fluorite is preferably ≥75wt%; the amount of the fluorite added is preferably 15-25wt% of the amount of the active lime added, specifically 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt% or 25wt%.
[0046] In the method provided by the present invention, in step B), after adding siliceous refining slag, active lime and fluorite, the flow rate of the argon gas can be specifically adjusted to 1.5NL / min, 1.6NL / min, 1.7NL / min, 1.8NL / min, 1.9NL / min, 2NL / min, 2.1NL / min, 2.2NL / min, 2.3NL / min, 2.4NL / min or 2.5NL / min per ton of steel.
[0047] In the method provided by the present invention, in step B), the target temperature of the refining is preferably 1560-1580°C, specifically 1560°C, 1565°C, 1570°C, 1575°C or 1580°C.
[0048] In the method provided by the present invention, in step B), when the temperature of the molten steel is specifically the target temperature +20°C, +21°C, +22°C, +23°C, +24°C, +25°C, +26°C, +27°C, +28°C, +29°C or +30°C, the flow rate of the argon blowing is adjusted to 4-5NL / min per ton of steel.
[0049] In the method provided by the present invention, in step B), when the temperature of the molten steel is the target temperature + 20 to 30°C, the flow rate of the argon gas blowing can be specifically adjusted to 4NL / min, 4.1NL / min, 4.2NL / min, 4.3NL / min, 4.4NL / min, 4.5NL / min, 4.6NL / min, 4.7NL / min, 4.8NL / min, 4.9NL / min or 5NL / min per ton of steel.
[0050] In the method provided by the present invention, in step B), after the flow rate of argon blowing is adjusted to 4-5NL / min per ton of steel, the bottom blowing time of argon gas at this flow rate can be specifically 5min, 5.5min, 6min, 6.5min, 7min, 7.5min, 8min, 8.5min, 9min, 9.5min or 10min.
[0051] In the method provided by the present invention, in step B), after the bottom blowing of argon for 5 to 10 minutes, the binary basicity of the refined slag in the ladle can be specifically 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3 or 2.4. In the present invention, the binary basicity refers to the ratio of CaO / SiO2 (the ratio of the weight percentages of CaO and SiO2 in the refined slag, respectively).
[0052] In the method provided by the present invention, in step C), during the entire process of vacuum treatment, the lifting gas flow rate can be specifically controlled at 9NL / min, 9.5NL / min, 10NL / min, 10.5NL / min, 11NL / min, 11.5NL / min, 12NL / min, 12.5NL / min or 13NL / min per ton of steel.
[0053] In the method provided by the present invention, in step C), during the whole process of vacuum treatment, the vacuum degree can be specifically controlled to be 10Pa, 20Pa, 30Pa, 40Pa, 50Pa, 60Pa, 70Pa, 80Pa, 90Pa or 100Pa.
[0054] In the method provided by the present invention, in step C), the alloying treatment is carried out after the vacuum treatment for 15 min, 15.5 min, 16 min, 16.5 min, 17 min, 17.5 min, 18 min, 18.5 min or 19 min.
[0055] In the method provided by the present invention, in step C), the time for continuing the vacuum treatment is preferably 5 to 10 minutes, specifically 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes.
[0056] In the method provided by the present invention, in step C), after breaking the vacuum, the argon blowing flow rate can be specifically adjusted to 0.5NL / min, 0.55NL / min, 0.6NL / min, 0.65NL / min, 0.7NL / min, 0.75NL / min or 0.8NL / min per ton of steel.
[0057] In the method provided by the present invention, in step C), after breaking the vacuum, the bottom blowing time of argon is preferably 3 to 10 minutes, specifically 3 minutes, 3.5 minutes, 4 minutes, 4.5 minutes, 5 minutes, 5.5 minutes, 6 minutes, 6.5 minutes, 7 minutes, 7.5 minutes, 8 minutes, 8.5 minutes, 9 minutes, 9.5 minutes or 10 minutes.
[0058] In the method provided by the present invention, in step C), the outlet temperature of the molten steel is preferably 1540-1560°C, specifically 1540°C, 1545°C, 1550°C, 1555°C or 1560°C.
[0059] The method provided by the present invention adopts a relatively low binary basicity of the refining slag in the ladle during the LF refining process, avoids the increase of the rating of brittle inclusions of types B, D, and Ds, and controls the inclusions of type C, and then utilizes the thermodynamic principle that high temperature is beneficial to the desulfurization of molten steel and the kinetic principle that strong stirring is beneficial to the desulfurization of molten steel, and at the end of the LF refining heating, the molten steel is made to reach a higher temperature and a large argon flow rate is used to strongly stir the molten steel and the refining slag in the ladle, so as to effectively remove sulfur from the steel. Experimental results show that the method provided by the present invention can control the S content of the finished rail steel product to be less than or equal to 0.008%, make the manganese sulfide inclusions dispersedly distributed, and ensure that the sulfide inclusion rating of the steel is less than or equal to level 2.5.
[0060] For the purpose of greater clarity, the invention is described in detail through the following examples.
[0061] Example 1
[0062] A) Converter smelting:
[0063] Molten iron with an S content of 0.018wt% was added to the converter, and 130t converter smelting was carried out at a smelting temperature of 1630°C. The carbon content of the molten steel at the end of smelting was 0.10wt% and the sulfur content was 0.017wt%. After the converter smelting was completed, alloys and carburizers required for steel grades such as ferrosilicon and ferromanganese were added during the steel tapping process. When the steel was tapped to 45t, 300kg of active lime (CaO content 85wt%) was added to the ladle.
[0064] B) LF furnace refining:
[0065] The molten steel is sent to the LF furnace for refining, and 200kg of siliceous refining slag (SiO2 content 45wt%, CaO content 40wt%), 600kg of active lime (CaO content 85wt%), and 120kg of fluorite (CaF2 content 75wt%) are added to the ladle in sequence, and the flow rate of argon blowing is adjusted to 2.5NL / min per ton of steel, and the molten steel is heated and refined; the target temperature for refining is set to 1560°C, and when the molten steel temperature is the target temperature+30°C, heating is stopped, and the flow rate of argon blowing is adjusted to 5.0NL / min per ton of steel. Argon is bottom blown for 10min at this flow rate, and then the binary basicity of the refined slag in the ladle is measured to be 2.3. When the molten steel temperature meets the target requirement, argon blowing is stopped and the molten steel leaves the station.
[0066] C) RH vacuum treatment:
[0067] The molten steel is sent to the RH vacuum treatment process for vacuum treatment. During the entire process of vacuum treatment, the lifting gas flow rate is controlled to be 12.5NL / min per ton of steel and the vacuum degree is 90Pa. After 19 minutes of vacuum treatment, the vacuum degree is maintained and then alloy is added for alloying treatment. After alloying, the vacuum cycle treatment is continued for 5 minutes until the composition is uniform and the vacuum is broken. Then, the argon blowing flow rate is adjusted to 0.55NL / min per ton of steel for bottom blowing of argon for 5 minutes. At this time, the measured temperature of the molten steel is 1545℃ and the molten steel leaves the station.
[0068] D) Continuous casting and rolling:
[0069] The molten steel is sent to the continuous casting process to produce 280×380mm large square continuous casting billet products; the continuous casting billet products are produced into 60kg / m rail steel through the rolling process.
[0070] By testing the steel rail produced by the method provided in this embodiment, the sulfur content of the steel rail produced by the process is 0.008%, and the ratings of non-metallic inclusions (GB / T 10561-2023) are as follows: Class B inclusion rating 0.5, Class D inclusion rating 1.0, Class Ds inclusion rating 0.5, Class A inclusion rating 2.5, Class C inclusion rating 0, and T[O] average 9.5×10 -6 .
[0071] Example 2
[0072] A) Converter smelting:
[0073] Molten iron with an S content of 0.011wt% was added into the converter, and 130t converter smelting was carried out at a smelting temperature of 1660°C. The carbon content of the molten steel at the end of smelting was 0.14wt% and the sulfur content was 0.011wt%. After the converter smelting was completed, alloys and carburizers required for steel grades such as ferrosilicon and ferromanganese were added during the steel tapping process. When the steel was tapped to 45t, 300kg of active lime (CaO content 85wt%) was added into the ladle.
[0074] B) LF furnace refining:
[0075] The molten steel is sent to the LF furnace for refining, and 450kg of siliceous refining slag (SiO2 content 45wt%, CaO content 40wt%), 350kg of active lime (CaO content 85wt%), and 80kg of fluorite (CaF2 content 75wt%) are added to the ladle in turn, and the flow rate of argon blowing is adjusted to 2.0NL / min per ton of steel, and the molten steel is heated and refined; the target temperature for refining is set to 1580°C, and when the molten steel temperature is the target temperature+25°C, heating is stopped, and the flow rate of argon blowing is adjusted to 4.0NL / min per ton of steel. Argon is bottom blown at this flow rate for 7min, and then the binary basicity of the refined slag in the ladle is measured to be 2.0. When the molten steel temperature meets the target requirement, argon blowing is stopped and the molten steel leaves the station.
[0076] C) RH vacuum treatment:
[0077] The molten steel is sent to the RH vacuum treatment process for vacuum treatment. During the entire process of vacuum treatment, the lifting gas flow rate is controlled to be 10NL / min per ton of steel and the vacuum degree is 70Pa. After 17 minutes of vacuum treatment, the vacuum degree is maintained and then alloy is added for alloying treatment. After alloying, the vacuum cycle treatment is continued for 7 minutes until the composition is uniform and the vacuum is broken. Then, the argon blowing flow rate is adjusted to 0.70NL / min per ton of steel for bottom blowing of argon for 7 minutes. At this time, the measured temperature of the molten steel is 1555℃ and the molten steel leaves the station.
[0078] D) Continuous casting and rolling:
[0079] The molten steel is sent to the continuous casting process to produce 280×380mm large square continuous casting billet products; the continuous casting billet products are produced into 60kg / m rail steel through the rolling process.
[0080] By testing the steel rail produced by the method provided in this embodiment, the sulfur content of the steel rail produced by the process is 0.006%, the rating of non-metallic inclusions is 0.5 for Class B inclusions, 0.5 for Class D inclusions, 0.5 for Class Ds inclusions, 1.5 for Class A inclusions, 1.0 for Class C inclusions, and the average T[O] is 6.0×10 -6 .
[0081] Example 3
[0082] A) Converter smelting:
[0083] Molten iron with an S content of 0.004wt% was added into the converter, and 130t converter smelting was carried out at a smelting temperature of 1645°C. The carbon content of the molten steel at the end of smelting was 0.06wt% and the sulfur content was 0.005wt%. After the converter smelting was completed, alloys and carburizers required for steel grades such as ferrosilicon and ferromanganese were added during the steel tapping process. When the steel was tapped to 45t, 300kg of active lime (CaO content 85wt%) was added into the ladle.
[0084] B) LF furnace refining:
[0085] The molten steel is sent to the LF furnace for refining, and 700kg of siliceous refining slag (SiO2 content 45wt%, CaO content 40wt%), 300kg of active lime (CaO content 85wt%), and 50kg of fluorite (CaF2 content 75wt%) are added into the ladle in turn, and the flow rate of argon blowing is adjusted to 1.5NL / min per ton of steel, and the molten steel is heated and refined; the target temperature for refining is set to 1570℃, and when the molten steel temperature is the target temperature+20℃, heating is stopped, and the flow rate of argon blowing is adjusted to 4.5NL / min per ton of steel. Argon is bottom blown for 5min at this flow rate, and then the binary basicity of the refined slag in the ladle is measured to be 1.7. When the molten steel temperature meets the target requirement, argon blowing is stopped and the molten steel leaves the station.
[0086] C) RH vacuum treatment:
[0087] The molten steel is sent to the RH vacuum treatment process for vacuum treatment. During the entire process of vacuum treatment, the lifting gas flow rate is controlled to be 9NL / min per ton of steel and the vacuum degree is 50Pa. After 16 minutes of vacuum treatment, the vacuum degree is maintained, and then alloy is added for alloying treatment. After alloying, the vacuum cycle treatment is continued for 6 minutes, and the vacuum is broken when the composition is uniform. Then, the argon blowing flow rate is adjusted to 0.80NL / min per ton of steel for bottom blowing of argon for 6 minutes. At this time, the measured temperature of the molten steel is 1550°C, and the molten steel leaves the station.
[0088] D) Continuous casting and rolling:
[0089] The molten steel is sent to the continuous casting process to produce 280×380mm large square continuous casting billet products; the continuous casting billet products are produced into 60kg / m rail steel through the rolling process.
[0090] By testing the steel rail produced by the method provided in this embodiment, the sulfur content of the steel rail produced by the process is 0.004%, the ratings of non-metallic inclusions are B-type inclusions rating 0, D-type inclusions rating 0, Ds-type inclusions rating 0, A-type inclusions rating 1.0, C-type inclusions rating 1.5, and T[O] average 7.0×10 -6 .
[0091] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for controlling non-metallic inclusions in rail steel, It is characterized in that The following steps are involved: A) Converter smelting: Adding molten iron with a sulfur content of ≤0.02wt% into the converter to carry out converter smelting, and controlling the carbon content of the molten steel at the end of the smelting to be 0.03-0.15wt%; adding alloys and carburizers required for the steel grade into the ladle during the steel tapping process after the converter smelting, and adding active lime when the steel tapping reaches 30-40%; B) LF furnace refining: After completing the treatment of step A), the ladle is sent to the LF furnace for refining, and siliceous refining slag, active lime and fluorite are added to the ladle in turn, and the flow rate of argon blowing is adjusted to 1.5-2.5NL / min per ton of steel, and the molten steel is heated and refined. When the molten steel temperature is the target temperature + 20-30°C, the flow rate of argon blowing is adjusted to 4-5NL / min per ton of steel. At this flow rate, argon is blown at the bottom for 5-10 minutes. At this time, the binary basicity of the refined slag in the ladle is 1.6-2.
4. When the molten steel temperature meets the target requirements, argon blowing is stopped and the molten steel is discharged; C) RH vacuum treatment: After the molten steel treated in step B) enters the station, the molten steel is subjected to RH vacuum treatment; during the entire process of vacuum treatment, the lifting gas flow rate is controlled to be 9-13NL / min per ton of steel, and the vacuum degree is ≤100Pa; after vacuum treatment for 15-19min, the vacuum degree is maintained, and then alloy is added for alloying treatment; after alloying, the vacuum treatment is continued for more than 5min to make the composition uniform, and the vacuum is broken; then, the bottom argon blowing is carried out for more than 3min under the condition of adjusting the blowing argon flow rate to 0.5-0.8NL / min per ton of steel, and the molten steel exits the station; D) Continuous casting and rolling: The molten steel treated in step C) is continuously cast, and then the obtained continuously cast billet is rolled to obtain rail steel.
2. The control method according to claim 1, It is characterized in that In step A), active lime is added when the steel tapping reaches 35%.
3. The control method according to claim 1, It is characterized in that In step A), the amount of active lime added is 1.5-3.5 kg per ton of molten steel.
4. The control method according to claim 1, It is characterized in that In step A), the CaO content of the active lime is ≥85wt%.
5. The control method according to claim 1, It is characterized in that In step B), the amount of the siliceous refined slag added is 1.5-6 kg per ton of molten steel.
6. The control method according to claim 1, It is characterized in that In step B), the SiO 2 The content is 30-50wt%, and the CaO content is 30-45wt%.
7. The control method according to claim 1, It is characterized in that In step B), the amount of active lime added is 2.5-4.5 kg per ton of molten steel.
8. The control method according to claim 1, It is characterized in that In step B), the CaO content of the active lime is ≥85wt%.
9. The control method according to claim 1, It is characterized in that In step B), the amount of fluorite added is 15-25wt% of the amount of active lime added.
10. The control method according to claim 1, It is characterized in that In step B), the CaF 2 Content ≥75wt%.