Marine work steel with excellent core low-temperature impact toughness and manufacturing method thereof

Through specific chemical composition and manufacturing processes, the problem of poor impact toughness and thickness direction uniformity of the core of thick-specific steel plates is solved, and the offshore steel plate with excellent high strength, low-temperature toughness and thickness direction performance is achieved, which is suitable for strict marine engineering and other rigorous projects. Application occasion.

CN118957418APending Publication Date: 2024-11-15NANJING IRON & STEEL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410818938.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to improve the impact toughness of the center and the uniformity of the thickness direction performance in thick-spec steel plates. Especially in applications such as marine engineering, bridge structures and high-rise buildings, structural failure is prone to occur when the steel plates are subjected to stress in the thickness direction. .

Method used

Specific chemical composition combinations and manufacturing processes are adopted, including directional molded blanks, multi-channel heat treatment and quenching processes, with specific components such as C: 0.08-0.14%, Si: 0.10-0.50%, Mn: 0.75-1.80%, Cu: 0.10 -0.50%, Ni: 1.4-1.85%, Cr: 0.50-0.95%, Mo: 0.10-0.55%, Al: 0.010-0.060%, Nb: 0.010-0.060%, P: 0.010% or less, S: 0.005% or less , N: below 0.0080%, combined with elements such as Ti, V, B, Ca, etc., the performance uniformity and low-temperature toughness of the steel plate in the thickness direction are ensured through casting billet smelting, heating, rolling, quenching and tempering processes.

Benefits of technology

It improves the performance uniformity of thick plates, achieves excellent low-temperature toughness and strong toughness matching, yield strength reaches 690MPa level, maximum thickness reaches 180mm, low-temperature impact toughness exceeds 100J, meets the requirements of Z35 level, and is suitable for structural applications that withstand stress in the thickness direction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses maritime work steel with excellent core low-temperature impact toughness, which is characterized by comprising the following chemical components in percentage by mass: 0.08 to 0.14 percent of C, 0.10 to 0.50 percent of Si, 0.75 to 1.80 percent of Mn, 0.10 to 0.50 percent of Cu, 1.4 to 1.85 percent of Ni, 0.50 to 0.95 percent of Cr, 0.10 to 0.55 percent of Mo, 0.010 to 0.060 percent of Al, 0.010 to 0.060 percent of Nb, less than 0.010 percent of P, less than 0.005 percent of S, less than 0.0080 percent of N and the balance of Fe and inevitable impurities. The manufacturing method comprises the steps of casting blank smelting, heating, rolling, heating, rolling, quenching and tempering. According to the method, the uniformity of the performance of the thick plate is improved, the 690MPa-grade extra-thick ultrahigh-strength steel plate with the thickness of 130-180mm is excellent in low-temperature toughness and good in obdurability matching, the yield strength is greater than or equal to 690Mpa, and the impact toughness at the position of 1 / 2 of the thickness of the plate at the temperature of-40 DEG C is 70% or above of the impact toughness at the position of 1 / 4 of the thickness of the plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a marine engineering steel with excellent core low-temperature impact toughness and a manufacturing method thereof, and in particular to a marine engineering steel suitable for use in marine engineering, bridge structures, high-rise buildings and other application occasions, which require the steel plate to withstand a certain stress structure in the thickness direction. Background Art

[0002] With the development of my country's industrial economy, the requirements for high-grade and high-performance steels have gradually increased, which has driven the research and development of domestic high-performance steels into a new stage. Among them, bridge structures, high-rise buildings, offshore platforms and hull structures usually use low-alloy high-strength steels. Since the application of the above structures requires the steel plates to withstand certain stresses in the thickness direction, such as poor core impact and layer tearing resistance of the steel plates, it is easy to cause structural damage. Therefore, these harsh engineering environments have put forward higher requirements for the uniformity of the thickness performance of the steel plates: thick-gauge steel plates are required to have certain strength and good uniformity of performance in the thickness direction.

[0003] Since the center segregation and center looseness caused by the billet are difficult to eliminate in the subsequent rolling, coupled with the uneven organization of the thick plate rolling and cooling process, the uniformity of the performance in the thickness direction of the steel plate is poor, especially the core impact is difficult to meet the requirements. The traditional process uses complex pure steel technology, such as rare earth treatment, Zr treatment, etc., but it is difficult to achieve; or normalizing heat treatment is used, but in order to compensate for the strength loss of the organizational changes after normalizing heat treatment, a large amount of micro-alloying elements need to be added; or offline quenching and tempering process is used, but because offline quenching and tempering treatment requires expensive equipment such as quenching machines, two processes of reheating and quenching are added, which correspondingly increases the production cycle and production cost, and it is impossible for steel mills that are not equipped with offline quenching and tempering production lines to produce. This restricts the improvement of the impact toughness of the core of thick-gauge steel plates. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a production method for steel for key engine fasteners with 15.8 grade ultra-high cycle fatigue performance in view of the shortcomings of the above prior art.

[0005] The technical solution of the present invention to solve the above technical problems is: a marine engineering steel with excellent low-temperature impact toughness in the core, characterized in that: the chemical composition mass percentage is: C: 0.08-0.14%, Si: 0.10-0.50%, Mn: 0.75-1.80%, Cu: 0.10-0.50%, Ni: 1.4-1.85%, Cr: 0.50-0.95%, Mo: 0.10-0.55%, Al: 0.010-0.060%, Nb: 0.010-0.060%, P: less than 0.010%, S: less than 0.005%, N: less than 0.0080%, and the balance is Fe and unavoidable impurities.

[0006] The present invention further defines the scheme:

[0007] Preferably, it also includes one or more of the components Ti, V, B and Ca.

[0008] Preferably, the mass percentage of Ti is 0.005-0.030%, the mass percentage of V is 0.001-0.10%, the mass percentage of B is less than 0.0030%, and the mass percentage of Ca is less than 0.0050%.

[0009] Preferably, the marine engineering steel adopts directional die casting billet, and the billet size is 620-630mm.

[0010] Preferably, the billet is heated to a temperature of 1100-1220°C, the cumulative rolling rate in the austenite recrystallization temperature range during hot rolling is above 40%, and the final cooling temperature is cooled to below 800°C.

[0011] Preferably, the above-mentioned method for manufacturing marine engineering steel comprises ingot smelting→heating→rolling→heating→rolling→quenching→tempering.

[0012] Preferably, the ingot smelting specifically includes:

[0013] (1) Smelting: molten iron charge ≥ 50 tons, steel tapping P ≤ 0.009%, steel tapping c ≥ 0.08%, steel tapping temperature 1600-1670°C, adding aluminum-containing raw materials for precipitation deoxidation;

[0014] (2) LF refining: using aluminum shot, deoxidation slag-making agent and other diffusion deoxidation, refining time ≥ 30min;

[0015] (3) When the high vacuum degree is ≤1.0mbar, the holding time is ≥20min, and the hydrogen content is less than 2ppm; after the vacuum is finished, static stirring is not less than 12min after the wire feeding is finished; the vacuum furnace hanging bag temperature is 1570-1584℃; after the static stirring time reaches the requirement and the temperature is appropriate, the hanging bag is molded;

[0016] (4) Die casting: The cross-section of the ingot is 620X2500mm, the superheat of the tundish is controlled at 20℃~40℃, the directional cooling mode is adopted, and the ingot stack is slowly cooled for 72h;.

[0017] Preferably, the rolling is specifically as follows: heating the ingot before rolling, the heating temperature is 1150-1250°C, the soaking time is 30-60min, the steel-out rolling temperature is 950-1100°C, the single pressing amount of the first 5 passes is ≥40mm, one-stage rolling, weak cooling after rolling to a thickness of 130mm-180mm, and the red-returning temperature is 780-820°C.

[0018] Preferably, the quenching includes primary quenching and secondary quenching, wherein:

[0019] The primary quenching temperature is 910-930°C, the furnace time is calculated as 1.0-2.0min / mm+(10-180min), and the furnace is quenched to room temperature after being taken out of the furnace;

[0020] Secondary quenching, quenching temperature 900 ~ 920 ℃, furnace time is calculated as 1.0 ~ 2.0min / mm + (10 ~ 180min), water quenching to room temperature after taking out of the furnace.

[0021] Preferably, in the tempering process, the tempering temperature is 580-680° C., the time in the furnace is calculated as 1.0-3.0 min / mm+(10-180 min), and air cooling is performed after the furnace is taken out.

[0022] The chemical components of the steel of the present invention are further described as follows:

[0023] C is a traditional strengthening element for steel, but it is very harmful to toughness and weldability. It has good weldability when the carbon content is less than 0.1%. With the development of microalloying and controlled rolling and controlled cooling technologies, the carbon content can be reduced while maintaining its high strength and toughness. However, when the carbon content of steel is less than 0.01%, the grain boundaries are weakened due to the reduction of interstitial carbon atoms and the precipitation of Nb, C, and N, making the grain boundaries in the heat-affected zone relatively brittle. Based on comprehensive performance, the carbon content range is set at 0.04% to 0.14%.

[0024] Si is effective as a deoxidizing element and a strengthening element, so it is contained in an amount of 0.10% or more. If the Si content exceeds 0.50%, the HAZ toughness greatly deteriorates, so the Si content is made 0.5% or less.

[0025] Mn mainly plays a role in solid solution strengthening. Under the same carbon content, as the manganese content increases, the strength increases. Manganese also plays a role in reducing the phase transition temperature and helps to refine the grains, so manganese is an indispensable element. However, if the manganese content is too high, the toughness will be reduced, resulting in serious banded structure of the steel plate and enhanced anisotropy. Therefore, the content of Mn is set to 0.75-1.8%.

[0026] Cu can improve the strength and toughness of the base material by adding Cu, so it is contained in an amount of 0.10% or more. However, if the Cu content is too high, HAZ toughness and weldability deteriorate, so 0.50% is made the upper limit.

[0027] Ni can effectively improve the low temperature toughness and corrosion resistance of steel, but as the nickel content increases, the production cost will increase significantly. The nickel content of the present invention is controlled at 1.4-1.85%.

[0028] Cr is one of the important elements for improving the hardenability of steel plates. For steel plates with extra-thick specifications, it is necessary to improve the hardenability of the steel plates by adding more Cr elements to compensate for the strength loss caused by the thickness. While improving the strength of the steel plates, it also improves the uniformity of the performance of the steel plates in the thickness direction. Cr can also inhibit the transformation of proeutectoid ferrite and pearlite, which is conducive to obtaining acicular ferrite structure. Once excessive Cr and Mn are added to the steel plate at the same time, it will lead to the formation of low-melting-point Cr-Mn composite oxides, which will cause the steel plate to form surface cracks during hot working and seriously deteriorate the welding performance of the steel plate. For this reason, the Cr content in the technical solution of the present invention should be limited to the range of 0.05% to 0.95%.

[0029] Al is an element added to steel for deoxidation. After complete deoxidation, Al reduces the content of O in the steel plate to improve the aging performance of the steel plate. In addition, adding an appropriate amount of Al is also beneficial to grain refinement, thereby improving the strength and toughness of the steel. Therefore, the content of Al in the steel plate with high crack arresting performance in the present invention is limited to 0.01-0.06%.

[0030] Nb is an important element in the present invention. In order to form a predetermined aspect ratio of the original austenite grains, rolling in the non-recrystallized austenite region is required. Nb is an element effective for expanding the non-recrystallized temperature region, and increasing the rolling temperature also helps to improve productivity. In order to obtain this effect, it is necessary to contain 0.010% or more. However, when the Nb content exceeds 0.060%, the HAZ toughness and weldability are reduced, so the Nb content is set to 0.060% or less.

[0031] P is one of the impurity elements. In order to stably ensure the HAZ toughness, the P content is limited to 0.010% or less.

[0032] S is one of the impurity elements. In order to stably ensure the properties of the base material and the HAZ toughness, the S content can be limited to 0.010% or less.

[0033] N combines with Al in steel to adjust the grain size during rolling and strengthen the steel. However, if N exceeds 0.0080%, the toughness deteriorates, so it is made 0.0080% or less.

[0034] Ti, when contained in a small amount, forms nitrides, carbides or carbonitrides, which has the effect of refining the grains and improving the toughness of the base material. This effect is obtained by containing 0.005% or more, but if it exceeds 0.030%, the toughness of the base material and the weld heat affected zone will decrease, so it is set to 0.005-0.030%.

[0035] Mo is an element that improves the hardenability of steel. It directly contributes to the improvement of strength after rolling, and can be contained to improve toughness, high temperature strength or weather resistance. These effects are exerted by containing 0.01% or more, but excessive inclusion will deteriorate toughness and weldability, so it is preferred to set the upper limit to 0.55%.

[0036] V is an element that improves the strength of steel by precipitation strengthening in the form of V (CN), and this effect is exerted by containing 0.001% or more. However, when containing more than 0.100%, the toughness is reduced. Therefore, when V is contained, it is preferably set in the range of 0.001 to 0.100%.

[0037] B may be contained as an element for improving the hardenability of steel in a trace amount, but if contained in an amount exceeding 0.0030%, the toughness of the weld portion is reduced, so when B is contained, it is preferably contained in an amount of 0.0030% or less.

[0038] Ca refines the structure of the weld heat affected zone to improve toughness, and even if contained, the effects of the present invention are not impaired. Therefore, it can be contained as needed. However, when contained excessively, coarse inclusions are formed to deteriorate the toughness of the base material. Therefore, when contained, the upper limit of the content is preferably set to 0.0050%.

[0039] The beneficial effects of the present invention are as follows: the present invention improves the uniformity of thick plate performance. The obtained steel plate has excellent low-temperature toughness, good strength-toughness matching, and is 130-180mm thick and 690MPa-grade ultra-thick ultra-high-strength steel plate, the maximum thickness of the steel plate reaches 180mm, the yield strength reaches 690MPa, the elongation is ≥18%, the low-temperature impact KV2 (-40℃)>100J, and the Z-direction performance is excellent and meets the Z35 level requirements. At the same time, the present invention adopts directional die casting billet, the billet size is 620-630mm, the yield strength is ≥690Mpa, and the -40℃ impact toughness at 1 / 2 of the plate thickness is more than 70% of the impact toughness at 1 / 4 of the plate thickness, which meets the application occasions where the steel plate is required to withstand a certain stress structure in the thickness direction. DETAILED DESCRIPTION

[0040] Implementation Case 1

[0041] The present embodiment provides a marine engineering steel with excellent low-temperature impact toughness in the core, which is an EH690 grade extra-thick steel plate, and its chemical composition and mass percentage are as follows: C: 0.12%, Si: 0.21%, Mn: 1.40%, P: 0.009%, S: 0.002%, Ni: 1.53%, Cr: 0.70%, Cu: 0.23%, Mo: 0.30%, Nb: 0.020%, V: 0.030%, Ti: 0.010%, Al: 0.020%, and the rest are Fe and unavoidable impurities.

[0042] The manufacturing method includes smelting of ingot → heating → rolling → heating → rolling → quenching → tempering, wherein

[0043] Ingot smelting: molten iron loading ≥ 50 tons, the S content of the molten iron is controlled to be 0.003% after desulfurization, the tapping P ≤ 0.009%, the tapping c ≥ 0.08%, the tapping temperature is 1600°C, and aluminum-containing raw materials are added for precipitation deoxidation;

[0044] (2) LF refining: using aluminum shot, deoxidation slag-making agent and other diffusion deoxidation, refining time 40min;

[0045] (3) When the high vacuum degree is ≤1.0mbar, the holding time is 20min, and the hydrogen content is less than 2ppm; after the vacuum is finished, static stirring is not less than 12min after the wire feeding is finished; the vacuum furnace hanging bag temperature is 1570℃; after the static stirring time reaches the requirement and the temperature is appropriate, the hanging bag is molded;

[0046] (4) Die casting: The cross section of the ingot is 620X2500mm, the superheat of the tundish is controlled at 30°C, the directional cooling mode is adopted, and the ingot stack is slowly cooled for 72h;

[0047] Rolling: The ingot is heated before rolling, the heating temperature is 1200℃, the soaking time is 430min, the steel-out rolling temperature is 1070℃, the first five passes have a single reduction of 41mm, one-stage rolling, the final rolling temperature is 940℃, and after rolling to a thickness of 130mm, it is weakly cooled and the red-returning temperature is 792℃; one-time quenching, the quenching temperature is 920℃, the furnace time is 210min, and the steel is water-quenched to room temperature after being discharged from the furnace;

[0048] Secondary quenching, quenching temperature 920℃, furnace time 210min, water quenching to room temperature after out of the furnace;

[0049] Tempering, tempering temperature 650℃, furnace time 360min, air cooling after out of the furnace.

[0050] Implementation Case 2

[0051] The present embodiment provides a marine engineering steel with excellent low-temperature impact toughness in the core, which is an EH690 grade extra-thick steel plate, and the chemical composition and mass percentage are as follows: C: 0.13%, Si: 0.42%, Mn: 1.60%, P: 0.010%, S: 0.001%, Ni: 1.78%, Cr: 0.80%, Cu: 0.36%, Mo: 0.45%, Nb: 0.040%, V: 0.030%, Ti: 0.015%, Al: 0.040%, and the rest are Fe and unavoidable impurities.

[0052] The manufacturing method includes smelting of ingot → heating → rolling → heating → rolling → quenching → tempering; wherein:

[0053] Ingot smelting: molten iron loading ≥ 50 tons, the S content of the molten iron is controlled to be 0.0023% after desulfurization, the tapping P ≤ 0.009%, the tapping c ≥ 0.08%, the tapping temperature is 1650°C, and aluminum-containing raw materials are added for precipitation deoxidation;

[0054] (2) LF refining: using aluminum shot, deoxidation slag-making agent and other diffusion deoxidation, refining time 40min;

[0055] (3) When the high vacuum degree is ≤1.0mbar, the holding time is 23min, and the hydrogen content is less than 2ppm; after the vacuum is finished, static stirring is not less than 12min after the wire feeding is finished; the vacuum furnace hanging bag temperature is 1577℃; after the static stirring time reaches the requirement and the temperature is appropriate, the hanging bag is molded;

[0056] (4) Die casting: The cross section of the ingot is 620X2500mm, the superheat of the tundish is controlled at 23°C, the directional cooling mode is adopted, and the ingot is stacked and slowly cooled for 72h;

[0057] Rolling, the heating temperature of the ingot is 1200℃, the soaking time is 53min, the steel-out rolling temperature is 1070℃, the first five passes are pressed with a single reduction of 42mm, one-stage rolling, the final rolling temperature is 960℃, and after rolling to the finished thickness, it is weakly cooled and the red-return temperature is 798℃;

[0058] One-time quenching, quenching temperature 920℃, furnace time 250min, water quenching to room temperature after out of the furnace;

[0059] Secondary quenching, quenching temperature 920℃, furnace time 250min, water quenching to room temperature after out of the furnace;

[0060] Tempering, tempering temperature 655℃, furnace time 460min, air cooling after out of the furnace.

[0061] Implementation Case 3

[0062] The present embodiment provides a marine engineering steel with excellent low-temperature impact toughness in the core, which is an EH690 grade extra-thick steel plate, and its chemical composition and mass percentage are as follows: C: 0.14%, Si: 0.49%, Mn: 1.60%, P: 0.008%, S: 0.002%, Ni: 1.82%, Cr: 0.85%, Cu: 0.40%, Mo: 0.50%, Nb: 0.050%, V: 0.040%, Ti: 0.018%, Al: 0.040%, and the rest are Fe and unavoidable impurities.

[0063] The manufacturing method includes smelting of ingot → heating → rolling → heating → rolling → quenching → tempering; wherein:

[0064] Ingot smelting: molten iron loading ≥ 50 tons, the S content of the molten iron is controlled to be 0.0003% after desulfurization, the tapping P ≤ 0.009%, the tapping c ≥ 0.08%, the tapping temperature is 1670°C, and aluminum-containing raw materials are added for precipitation deoxidation;

[0065] (2) LF refining: using aluminum shot, deoxidation slag-making agent and other diffusion deoxidation, refining time 45min;

[0066] (3) When the high vacuum degree is ≤1.0mbar, the holding time is 26min, and the hydrogen content is less than 2ppm; after the vacuum is finished, static stirring is not less than 12min after the wire feeding is finished; the vacuum furnace hanging bag temperature is 1584℃; after the static stirring time reaches the requirement and the temperature is appropriate, the hanging bag is molded;

[0067] (4) Die casting: The cross section of the ingot is 620X2500mm, the superheat of the tundish is controlled at 20°C, the directional cooling mode is adopted, and the ingot is stacked and slowly cooled for 72h;

[0068] Rolling, the heating temperature of the ingot is 1200℃, the soaking time is 62min, the steel tapping and rolling temperature is 1050℃, the first five passes are pressed with a single reduction of 43mm, one-stage rolling, the final rolling temperature is 960℃, and after rolling to the finished thickness, it is weakly cooled and the red-return temperature is 798℃;

[0069] One quenching, quenching temperature 920℃, furnace time 282min, water quenching to room temperature after out of the furnace;

[0070] Secondary quenching, quenching temperature 900℃, furnace time 282min, water quenching to room temperature after out of the furnace;

[0071] Tempering, tempering temperature 653℃, furnace time 540min, air cooling after out of the furnace.

[0072] The mechanical properties of the steel plates obtained in the above examples 1-3 are shown in Table 1.

[0073] Table 1

[0074]

[0075] It can be seen from Table 1 that the steel plate produced by the present invention mainly consists of bainite + martensite, with a maximum thickness of 180 mm and a compression ratio of >3.0; the yield strength reaches 690 MPa, the yield strength is 710-743 MPa, the tensile strength is 813-839 MPa, the elongation is ≥18%, and the low-temperature toughness KV2 (-40°C) reaches more than 100 J; the performance in the thickness direction is good, meeting the Z35 level requirements, and the comprehensive performance is excellent with good matching of strength and toughness.

[0076] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.

Claims

1. A marine engineering steel with excellent core low-temperature impact toughness, characterized in that: Its chemical composition by mass percentage is: C: 0.08-0.14%, Si: 0.10-0.50%, Mn: 0.75-1.80%, Cu: 0.10-0.50%, Ni: 1.4-1.85%, Cr: 0.50-0.95%, Mo: 0.10-0.55%, Al: 0.010-0.060%, Nb: 0.010-0.060%, P: less than 0.010%, S: less than 0.005%, N: less than 0.0080%, and the balance is Fe and unavoidable impurities.

2. The marine engineering steel with excellent core low-temperature impact toughness according to claim 1, characterized in that: It also includes one or more of the components Ti, V, B and Ca.

3. The marine engineering steel with excellent core low-temperature impact toughness according to claim 2, characterized in that: The mass percentage of Ti is 0.005-0.030%, the mass percentage of V is 0.001-0.10%, the mass percentage of B is less than 0.0030%, and the mass percentage of Ca is less than 0.0050%.

4. The marine engineering steel with excellent core low-temperature impact toughness according to claim 1, characterized in that: The marine engineering steel adopts directional die casting billet, and the billet size is 620-630mm.

5. The marine engineering steel with excellent core low-temperature impact toughness according to claim 3, characterized in that: The above-mentioned billet is heated to a temperature of 1100-1220°C, the cumulative rolling rate in the austenite recrystallization temperature range during hot rolling is more than 40%, and the final cooling temperature is cooled to less than 800°C.

6. A marine engineering steel with excellent core low-temperature impact toughness according to any one of claims 1 to 4, characterized in that: The above-mentioned offshore steel manufacturing method includes ingot smelting→heating→rolling→heating→rolling→quenching→tempering.

7. The method for manufacturing marine engineering steel with excellent core low-temperature impact toughness according to claim 5, characterized in that: The ingot smelting specifically includes: (1) Smelting: molten iron charge ≥ 50 tons, steel tapping P ≤ 0.009%, steel tapping c ≥ 0.08%, steel tapping temperature 1600-1670℃, adding aluminum-containing raw materials for precipitation deoxidation; (2) LF refining: using aluminum shot, deoxidation slag-making agent and other diffusion deoxidation, refining time ≥ 30min; (3) High vacuum degree ≤1.0mbar, holding time ≥20min, hydrogen content less than 2ppm; static stirring for no less than 12min after vacuum and wire feeding; vacuum furnace bag temperature 1570-1584℃ (liquidus 1504℃); static stirring time reaches the requirement, and the bag is molded for casting at the appropriate temperature; (4) Die casting: The cross section of the ingot is 620X2500mm, the superheat of the tundish is controlled at 20℃~40℃, and a directional cooling mode is adopted.

8. The method for manufacturing a marine engineering steel with excellent core low-temperature impact toughness according to claim 5, characterized in that: The rolling process is specifically as follows: heating the ingot before rolling, the heating temperature is 1150-1250°C, the soaking time is 30-60min, the steel-out rolling temperature is 950-1100°C, the first 5 passes have a single reduction of ≥40mm, one-stage rolling, after rolling to a thickness of 130mm-180mm, weak cooling, and the red-returning temperature is 780-820°C.

9. The method for manufacturing a marine engineering steel with excellent core low-temperature impact toughness according to claim 5, characterized in that: The quenching includes primary quenching and secondary quenching, wherein: The primary quenching temperature is 910-930℃, the furnace time is calculated as 1.0-2.0min / mm+ (10-180min), and the steel is water quenched to room temperature after being taken out of the furnace; Secondary quenching, quenching temperature 900 ~ 920 ℃, furnace time is calculated as 1.0 ~ 2.0min / mm + (10 ~ 180min), water quenching to room temperature after taking out of the furnace.

10. The method for manufacturing a marine engineering steel with excellent core low-temperature impact toughness according to claim 5, characterized in that: In the tempering process, the tempering temperature is 580-680°C, the time in the furnace is calculated as 1.0-3.0 min / mm + (10-180 min), and the steel is air-cooled after being taken out of the furnace.

Citation Information

Cited By

  • Rare earth W-Mo composite alloying 690MPa-grade extra-thick maritime work steel plate and preparation method thereof

    CN122327099A