Continuous annealing processing technology based on aluminum plate
Through visually guided robot clamping and electromagnetic induction heating, laser cleaning and jet cooling technology, the problems of manual handling, uneven heating and chemical cleaning and corrosion during continuous annealing of aluminum sheets are solved, and the efficient and safe annealing process of aluminum sheets is achieved .
Patent Information
- Application Number
- CN202411044385.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
During the continuous annealing process, existing aluminum sheets have problems such as manual handling, uneven heating and corrosion caused by chemical cleaning.
Vision-guided robots are used to accurately clamp and carry the aluminum plate, and electromagnetic induction heating and laser cleaning technology are used to heat and clean the aluminum plate with jet cooling.
It realizes safe and efficient handling, uniform heating, clean and corrosion-free aluminum plates, and improves the safety and performance of the annealing process of aluminum plates.
Smart Images

Figure CN118957458A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum plate annealing, in particular to a continuous annealing processing technology based on aluminum plate. Background Art
[0002] Aluminum sheet is a type of aluminum material. It is processed from aluminum ingot into plate-shaped aluminum products through plastic processing methods such as rolling, extrusion, stretching and forging. In order to ensure the final performance of the sheet, the finished product will also be annealed, solution treated, quenched, naturally aged and artificially aged.
[0003] Continuous annealing is relative to hood annealing. It is a production method in which the strip steel continuously passes through the annealing furnace. The annealing furnace is not sealed, and the strip steel is directly coiled without stopping. This production method allows the deformed grains to be transformed into uniform equiaxed grains, and eliminates work hardening and residual internal stress, so that the organization and performance of the steel can be restored to the state before cold deformation.
[0004] Aluminum plates generally go through cleaning, heating and cooling steps during continuous annealing. Existing aluminum plates have the following technical problems during continuous annealing:
[0005] Problem 1: Aluminum plates are often transported manually, which is dangerous.
[0006] Problem 2: The existing aluminum plate annealing heating mainly uses a preheating furnace, which has a good heating effect but easily leads to uneven heating;
[0007] Question three: Before annealing, the existing aluminum plate cleaning mainly relies on chemical cleaning methods, which mix chemicals with water to wipe the surface of the plate. Although it has a certain cleaning effect, it is easy to corrode the plate over a long period of use and is also harmful to employees. Summary of the invention
[0008] Technical issues solved
[0009] In view of the shortcomings of the prior art, the present invention provides a continuous annealing processing technology based on aluminum plates, which solves the following problems:
[0010] 1. Through visual guidance, the robot can accurately clamp the aluminum plate, solving the problem that many aluminum plates are transported manually, which is dangerous.
[0011] 2. Electromagnetic induction is used to heat the plate, which makes the heating more uniform. This solves the problem that the existing aluminum plate annealing heating mainly uses a preheating furnace, which has a good heating effect but easily leads to uneven heating.
[0012] 3. The surface of the plate is cleaned by laser cleaning, which solves the problem that the existing aluminum plate cleaning before annealing mainly relies on chemical cleaning. Chemical agents are mixed with water to wipe the surface of the plate. Although it has a certain cleaning effect, it is easy to corrode the plate after long-term use, and it is also harmful to employees.
[0013] Technical Solution
[0014] To achieve the above objectives, the present invention is implemented by the following technical scheme: Based on the continuous annealing processing technology of aluminum plate, the continuous annealing processing steps of the aluminum plate mainly include cleaning, heating and cooling, wherein:
[0015] The cleaning adopts laser cleaning, the heating method adopts electromagnetic induction heating, and the cooling adopts jet cooling.
[0016] The plate itself is grasped by a robot, which uses a clamp and a suction cup as the end effector and an auxiliary sensor to form a grasping system to complete operations such as sorting and handling of parts. The robot uses a double-arm robot.
[0017] The robot body is equipped with a visual system, which detects the appearance, length, width and thickness characteristics of the aluminum plate through a target detection algorithm. The target detection algorithm is divided into a traditional target detection algorithm and a target detection algorithm based on deep learning. The traditional target detection algorithm mainly takes manual features as the core and processes images using a sliding frame method. The way it processes images adopts a global search method from left to right and from top to bottom. The target detection network based on deep learning is designed based on a convolutional neural network to classify and locate objects. Currently, the commonly used classic convolutional neural networks are: Al exNet, Overfeat, GoogLeNet, VGG and ResNet.
[0018] Preferably, the visual system extracts candidate areas through a Selective Search clustering search algorithm. The number of extracted candidate areas is about 2000 according to the needs of the network. All areas are fixed to a certain size by cropping or scaling. CNN is used to extract features, and the extracted features are passed to a subsequent fully connected layer. The image features extracted from CNN are classified and redundant prior frames are removed. During the detection process, there will be multiple prior frames around the same object to detect it. It is necessary to select the most accurate one from these frames to obtain accurate location information of the target.
[0019] Preferably, the visual system obtains information mainly by relying on an industrial camera, and after obtaining accurate position information of the aluminum plate, controls the robot to move the aluminum plate to the cleaning equipment using a clamp and a suction cup.
[0020] Preferably, the aluminum plate is cleaned by laser cleaning, and a simulation is first performed. The ANSYS analysis software is used to simulate the temperature field distribution during the pulse laser cleaning of the aluminum plate, revealing the influence of the oxide film and substrate temperature on the removal morphology of the aluminum plate surface under the action of the laser. The temperature field changes of the oxide film and the aluminum plate substrate are determined when the laser spot diameter is 0.5mm-2mm, the pulse width is 50ns-200ns, the repetition frequency is 8kHz-11kHz, and the overlap rate is 20%-80%. The cleaning process pre-parameters in the simulation process are obtained: the optimal laser spot diameter is 0.5mm, the optimal laser pulse width is 50ns, the optimal repetition frequency is 8kHz, and the optimal spot overlap rate is 40%.
[0021] Preferably, in the laser cleaning process, Nd:YAG laser is used for cleaning with a laser power of 50W-110W and a cleaning speed of 1mm / s-20.7mm / s. As the cleaning speed continues to slow down, welding slag such as MgO and Al2O3 is gradually removed, and the oxygen content in the weld area reaches the lowest value at 5.2mm / s.
[0022] Preferably, electromagnetic induction heating is performed after the cleaning is completed, and in the electromagnetic induction heating step, the temperature of the electromagnetic induction heating is adjusted by controlling the output of the power supply.
[0023] Preferably, spray cooling is performed after the cleaning is completed, and the cooling part of the aluminum plate to be cooled is aligned with the coolant nozzle by a robot, and a guide plate is installed. The size of the guide plate is adjusted according to the size of the aluminum plate, and a flow channel for supplying coolant is opened inside the guide plate.
[0024] Preferably, the spray cooling insert selects sealant to smear the edge of the plate, and there are gaps on the plate that need to fill the gaps between the joint surfaces to form a uniform and stable continuous film with viscosity, viscoelasticity or peelability, thereby sealing between the joint surfaces of the various components of the equipment, so that the coolant cools the components that need to be cooled.
[0025] Preferably, the cooling liquid spray head before the injection cooling is inserted into the drainage groove opened inside the drainage plate, and under the action of an external force device, the cooling liquid is sprayed from the spray head, and the cooling liquid spraying speed is 0.8m / s. The external force device here is mainly a suction pump.
[0026] Preferably, the drying time of the sealant when applied is 2-3 minutes, the plate is automatically turned over by a robot during the cooling step, and the coolant is mainly composed of water, ethylene glycol and additives, and the additive is a corrosion inhibitor.
[0027] Beneficial Effects
[0028] The present invention provides a continuous annealing processing technology based on aluminum plates. It has the following beneficial effects:
[0029] 1. The plate itself is grasped by a robot, with a clamp and a suction cup as the end effector, and an auxiliary sensor forming a grasping system to complete operations such as sorting and handling of parts. The robot uses a two-arm robot, which can accurately clamp the aluminum plate through visual guidance. The visual system obtains information mainly through industrial cameras. After obtaining the accurate position information of the aluminum plate, the robot is controlled to use the clamp and suction cup to move the aluminum plate to the cleaning equipment.
[0030] 2. The aluminum plate of the present invention is cleaned by laser cleaning. During the laser cleaning process, Nd:YAG laser is used for cleaning. The laser power is 50W-110W and the cleaning speed is 1mm / s-20.7mm / s. As the cleaning speed continues to slow down, welding slag such as MgO and Al2O3 is gradually removed. At 5.2mm / s, the oxygen content in the weld area reaches the lowest value, which solves the problem that the existing aluminum plate cleaning before annealing mainly relies on chemical cleaning, in which chemical agents are mixed with water to wipe the surface of the plate. Although it has a certain cleaning effect, it is easy to corrode the plate after long-term use, and it is also harmful to employees.
[0031] 3. The present invention adopts electromagnetic induction heating, and the aluminum plate is placed in the induction coil to ensure good contact and proximity between the aluminum material and the coil so as to generate sufficient induction furnace. Then the power is turned on and the generator is started. The generator will emit high-frequency current to form a high-frequency magnetic field through the induction coil. This magnetic field will generate eddy currents inside the aluminum material, thereby causing the aluminum material to heat itself. The aluminum plate itself is a conductor, so the heating speed is fast and the energy utilization rate is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a specific process step diagram of annealing of the present invention;
[0033] Figure 2 It is a flow chart of the target detection algorithm of the present invention;
[0034] Figure 3 It is the robot control operation diagram of the present invention;
[0035] Figure 4 Specific parameter diagram of the robot of the present invention; DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Specific embodiment one:
[0038] like Figure 1-4 As shown, based on the continuous annealing process technology of aluminum sheet, the continuous annealing process steps of aluminum sheet mainly include cleaning, heating and cooling, among which:
[0039] Laser cleaning is used for cleaning, electromagnetic induction heating is used for heating, and jet cooling is used for cooling.
[0040] The plate itself is grasped by a robot, which uses a clamp and a suction cup as the end effector and uses auxiliary sensors to form a grasping system to complete operations such as sorting and handling of parts. A dual-arm robot is used.
[0041] The robot body is equipped with a visual system, which detects the appearance, length, width and thickness characteristics of the aluminum plate through the target detection algorithm. The target detection algorithm is divided into traditional target detection algorithm and target detection algorithm based on deep learning. Among them, the traditional target detection algorithm mainly takes manual features as the core, and processes the image with the sliding frame method. The way it processes pictures adopts a global search method from left to right and from top to bottom. The target detection network based on deep learning is designed based on convolutional neural networks to classify and locate objects. The commonly used classic convolutional neural networks are: AlexNet, Overfeat, GoogLeNet, VGG and ResNet.
[0042] In the deep learning object detection, according to the network processing process, it can be divided into two categories: one-stage and two-stage. The two-stage object detection algorithm was proposed before the one-stage object detection algorithm. The core of this algorithm is to extract candidate areas from the image first, and then perform classification detection. It abandons the traditional image processing technology and uses convolutional neural networks to extract image features. It uses clustering search algorithms to replace the sliding frame technology in traditional image technology to extract candidate areas.
[0043] The visual system extracts candidate areas through the Selective Search clustering search algorithm. The number of extracted candidate areas is about 2000 according to the needs of the network. All areas are fixed to a certain size by cropping or scaling. CNN is used to extract features and the extracted features are passed to the subsequent fully connected layer. The image features extracted by CNN are classified and redundant prior frames are removed. During the detection process, there will be multiple prior frames around the same object to detect it. It is necessary to select the most accurate one from these frames to obtain the accurate location information of the target.
[0044] The visual system mainly relies on industrial cameras to obtain information. After obtaining the accurate position information of the aluminum plate, the robot is controlled to use clamps and suction cups to move the aluminum plate to the cleaning equipment.
[0045] In the present invention, the robot can accurately clamp the aluminum plate through visual guidance. The specific target detection algorithm process is as follows: Figure 2 As shown, the robot arm is a serial robot arm, and the end grasping structure of the robot arm is driven by a permanent magnet linear stepper motor. Specific embodiment 2:
[0047] like Figure 1-4 As shown in the figure, the aluminum plate is cleaned by laser cleaning. First, a simulation is carried out. The ANSYS analysis software is used to simulate the temperature field distribution during the pulse laser cleaning of the aluminum plate, revealing the influence of the oxide film and substrate temperature on the removal morphology of the aluminum plate surface under the action of the laser. The temperature field changes of the oxide film and the aluminum plate substrate when the laser spot diameter is 0.5mm-2mm, the pulse width is 50ns-200ns, the repetition frequency is 8kHz-11kHz, and the overlap rate is 20%-80%. The cleaning process pre-parameters in the simulation process are as follows: the optimal laser spot diameter is 0.5mm, the optimal laser pulse width is 50ns, the optimal repetition frequency is 8kHz, and the optimal spot overlap rate is 40%.
[0048] During the laser cleaning process, Nd:YAG laser is used for cleaning with a laser power of 50W-110W and a cleaning speed of 1mm / s-20.7mm / s. As the cleaning speed continues to slow down, welding slag such as MgO and Al2O3 is gradually removed, and the oxygen content in the weld area reaches the lowest value at 5.2mm / s. Specific embodiment three:
[0050] like Figure 1-4 As shown, electromagnetic induction heating is performed after cleaning. In the electromagnetic induction heating step, the temperature of electromagnetic induction heating is adjusted by controlling the output of the power supply. In the overall scheme of the system, an open-loop control method is used to control the power supply. This method avoids the uncertainty in the temperature acquisition process. The specific process of electromagnetic induction is as follows:
[0051] Speed regulation: During the heating process, the frequency and current of the transformer are first adjusted to change the size and strength of the magnetic field, thereby controlling the speed of heating.
[0052] Heating: The high voltage current in the transformer is passed through the center magnetic pole to generate a strong magnetic field, and then the strong magnetic field is introduced into the outer magnetic pole, so that the object is subjected to the modulated electromagnetic force, thereby achieving heating.
[0053] Control: By changing the frequency and current in the transformer, the heating speed and heating accuracy can be controlled to achieve the desired heating effect.
[0054] The entire electromagnetic induction heating system is mainly composed of a power supply, a generator, an induction coil and a heater workpiece. The specific design is as follows:
[0055] Power supply: The electromagnetic induction heater needs to be connected to a power source to work. It uses AC power and the frequency can be selected according to specific needs.
[0056] Generator: It is the core part of the whole system, which can convert the electric energy of AC power into high-frequency AC power, generate high-frequency electromagnetic field, induce eddy current in the induction coil, and thus convert the electric energy into heat energy. The main structure of the generator includes energy transformer, full-bridge circuit, resonant capacitor, etc.
[0057] Induction coil: The induction coil is the executive component of the electromagnetic induction heater. It is made of copper tubes, copper plates, etc. and is placed on the upper and lower planes of the workpiece respectively. The high-frequency electromagnetic field generated can form eddy currents inside the workpiece and produce a thermal effect.
[0058] Heater workpiece: This is the object to be heated, usually a material with good conductivity, such as metal. When the heater workpiece is placed near the induction coil, the high-frequency current in the induction coil generates an alternating magnetic field.
[0059] In actual operation, the aluminum plate is placed in the induction coil to ensure good contact and proximity between the aluminum and the coil so as to generate sufficient induction furnace. Then the power is turned on and the generator is started. The generator will emit a high-frequency current to form a high-frequency magnetic field through the induction coil. This magnetic field will generate eddy currents inside the aluminum, causing the aluminum to heat itself. The aluminum plate itself is a conductor, so the heating speed is fast and the energy utilization rate is high. Specific embodiment four:
[0061] like Figure 1-4 As shown, after cleaning, spray cooling is performed. The robot aligns the cooling area of the aluminum plate with the coolant nozzle, and installs a guide plate. The size of the guide plate is adjusted according to the size of the aluminum plate, and a flow channel for supplying coolant is opened inside the guide plate.
[0062] The spray cooling insert selects sealant to apply to the edge of the plate. There are gaps on the plate that need to be filled in the gaps between the joint surfaces to form a uniform and stable continuous film with viscosity, viscoelasticity or peelability, thereby sealing the joint surfaces of the various parts of the equipment and allowing the coolant to cool the parts that need to be cooled.
[0063] Before the spray cooling, the coolant spray head is inserted into the drainage groove opened inside the drainage plate, and under the action of the external force device, the coolant is sprayed from the spray head. The speed of the coolant spray is 0.8m / s. The external force device here is mainly a suction pump.
[0064] The drying time when the sealant is applied is 2-3 minutes. The plate must be automatically flipped by a robot during the cooling step. The coolant is mainly composed of water, ethylene glycol and additives, and the additive is a corrosion inhibitor.
[0065] In the actual spray cooling process, according to the material, thickness, required cooling rate and final use of the aluminum plate, the appropriate spray cooling parameters should be set, including the temperature, flow rate, pressure of the cooling medium and the arrangement and spacing of the nozzles. Then, the spray cooling equipment should be started to spray the cooling medium evenly onto the surface of the aluminum plate in the form of a spray. Ensure that the spray range covers the entire aluminum plate and avoid local overheating or overcooling. During the spraying process, the spray angle and distance can be adjusted as needed to achieve the best cooling effect. During the spray cooling process, the temperature change and cooling effect of the aluminum plate should be monitored in real time. If uneven cooling or large temperature fluctuations are found, the spray parameters should be adjusted in time or the spray method should be changed. After the spray cooling is completed, the aluminum plate should be subjected to necessary follow-up treatment, such as cleaning the surface residue and checking the cooling effect to ensure that the aluminum plate achieves the expected cold zone effect and performance requirements.
[0066] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the statement "comprising a reference structure" do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0067] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. Continuous annealing technology based on aluminum sheet, characterized by: The aluminum plate continuous annealing process mainly includes cleaning, heating and cooling, wherein: The cleaning adopts laser cleaning, the heating method adopts electromagnetic induction heating, and the cooling adopts jet cooling. The plate itself is grasped by a robot, which uses a clamp and a suction cup as the end effector and an auxiliary sensor to form a grasping system to complete operations such as sorting and handling of parts. The robot uses a double-arm robot. The robot body is equipped with a visual system, which detects the appearance, length, width and thickness characteristics of the aluminum plate through a target detection algorithm. The target detection algorithm is divided into a traditional target detection algorithm and a target detection algorithm based on deep learning.
2. The continuous annealing process technology based on aluminum sheet according to claim 1 is characterized in that: The visual system extracts candidate areas through the Selective Search clustering search algorithm. The number of extracted candidate areas is about 2000 according to the needs of the network. All areas are fixed to a certain size by cropping or scaling. CNN is used to extract features, and the extracted features are passed to the subsequent fully connected layer. The image features extracted by CNN are classified and redundant prior frames are removed. During the detection process, there will be multiple prior frames around the same object to detect it. It is necessary to select the most accurate one from these frames to obtain accurate location information of the target.
3. The continuous annealing process based on aluminum sheet according to claim 1, characterized in that: The visual system mainly relies on industrial cameras to obtain information. After obtaining the accurate position information of the aluminum plate, the robot is controlled to use a clamp and a suction cup to move the aluminum plate to the cleaning equipment.
4. The continuous annealing process technology based on aluminum sheet according to claim 3 is characterized in that: The aluminum plate is cleaned by laser cleaning. First, a simulation is performed. ANSYS analysis software is used to simulate the temperature field distribution in the process of pulse laser cleaning the aluminum plate, revealing the influence of the oxide film and substrate temperature on the surface removal morphology of the aluminum plate under the action of the laser. The temperature field changes of the oxide film and the aluminum plate substrate are obtained when the laser spot diameter is 0.5mm-2mm, the pulse width is 50ns-200ns, the repetition frequency is 8kHz-11kHz, and the overlap rate is 20%-80%. The cleaning process pre-parameters in the simulation process are obtained: the optimal laser spot diameter is 0.5mm, the optimal laser pulse width is 50ns, the optimal repetition frequency is 8kHz, and the optimal spot overlap rate is 40%.
5. The continuous annealing process technology based on aluminum sheet according to claim 3 is characterized in that: In the laser cleaning process, Nd:YAG laser is used for cleaning with a laser power of 50W-110W and a cleaning speed of 1mm / s-20.7mm / s.
6. The continuous annealing process technology based on aluminum sheet according to claim 4, characterized in that: After the cleaning is completed, electromagnetic induction heating is performed. In the electromagnetic induction heating step, the temperature of the electromagnetic induction heating is adjusted by controlling the output of the power supply.
7. The continuous annealing process technology based on aluminum sheet according to claim 5, characterized in that: After the cleaning is completed, spray cooling is performed. The cooling part of the aluminum plate to be cooled is aligned with the cooling liquid nozzle by a robot, and a guide plate is installed. The size of the guide plate is adjusted according to the size of the aluminum plate, and a flow channel for supplying coolant is opened inside the guide plate.
8. The continuous annealing process based on aluminum sheet according to claim 7, characterized in that: The spray cooling insert selects sealant to smear the edge of the plate, and the gaps on the plate need to be filled up between the joint surfaces to form a uniform and stable continuous film with viscosity, viscoelasticity or peelability.
9. The continuous annealing process technology based on aluminum sheet according to claim 8, characterized in that: The cooling liquid spray head before the spray cooling is plugged into the drainage groove opened inside the drainage plate, and under the action of an external force device, the cooling liquid is sprayed from the spray head, and the speed of the cooling liquid spraying is 0.8m / s.
10. The continuous annealing process technology based on aluminum sheet according to claim 9, characterized in that: The drying time of the sealant when applied is 2-3 minutes. The plate is automatically turned over by a robot during the cooling step. The coolant is mainly composed of water, ethylene glycol and additives, and the additive is a corrosion inhibitor.