Capacitor film with excellent self-healing property and preparation method and application of capacitor

By depositing alumina or zinc oxide functional layer with high dielectric constant and wide energy bandgap on the surface of BOPP film, combined with plasma treatment and vacuum evaporation technology, the performance improvement of capacitor films under high temperature and high electric fields in the prior art is solved. The problem is that higher electrical performance and self-healing characteristics are achieved, and are suitable for industrial applications.

CN118957498APending Publication Date: 2024-11-15CHINA THREE GORGES CORPORATION
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410945817.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, high-insulating thin-layer deposition methods have many defects, high cost, slow deposition rate and low dielectric constant, resulting in limited performance improvement of polymer capacitor films under high temperature and high electric fields.

Method used

The evaporation technology is used to deposit alumina or zinc oxide functional layer on the surface of the BOPP film. By combining plasma treatment and vacuum evaporation, a functional layer with high dielectric constant and wide energy band gap is formed to improve the high-temperature electrical performance of the capacitor. and self-healing characteristics.

Benefits of technology

It significantly reduces the leakage current at high temperature and high fields, improves the high temperature electrical performance and self-healing characteristics of the capacitor, has low defect density, is suitable for industrial production, and improves the durability and working temperature of the capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957498A_ABST
    Figure CN118957498A_ABST
Patent Text Reader

Abstract

The invention relates to an excellent self-healing capacitor film and a preparation method and application of a capacitor thereof. The capacitor film comprises a dielectric film, a functional layer is arranged on the surface of the dielectric film, the dielectric film is a BOPP film, and the functional layer is an aluminum oxide layer or a zinc oxide layer. According to the preparation method of the capacitor film, the functional layers are evaporated on the two faces of the dielectric film through plasma and evaporation, and the high-temperature-resistant capacitor film with the self-healing capacity is formed. The capacitor film prepared by the invention has few surface defects and lower leakage current under high temperature and high field, and the metallized film capacitor formed by winding has more excellent self-healing characteristic. Moreover, the method can be matched with the production speed of the capacitor film, and is more suitable for industrial utilization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic film capacitors, and specifically relates to a preparation method and application of an excellent self-healing capacitor film and a capacitor thereof. Background Art

[0002] Patent CN108962596A discloses a method for preparing a high-temperature capacitor film based on atmospheric pressure low-temperature plasma deposition. A thin layer with high insulation performance is deposited on the surface of a polymer capacitor film by atmospheric pressure low-temperature plasma deposition technology. A thin layer with high insulation performance is introduced between the metal electrode and the polymer capacitor film. The thin layer with high insulation performance has a wide energy band gap and is used as a charge blocking layer, thereby effectively suppressing the leakage current formed by charge injection at the electrode under high temperature and high electric field, thereby improving the charging and discharging efficiency of the polymer capacitor film under high temperature and high electric field, and achieving the purpose of increasing its operating temperature. The method for depositing a high insulation performance layer in this patent is normal temperature plasma assisted chemical vapor deposition. The deposited high insulation performance layer has many defects, and the amount of argon used in the deposition process is high, resulting in limited improvement effect on the high temperature performance of the capacitor film, high cost, and slow deposition rate. In addition, the insulating layer material used in the patent is silicon dioxide, which has a low dielectric constant and limited effect on improving the high temperature performance of the capacitor film. Summary of the invention

[0003] In view of the problems existing in the prior art, in order to solve the above defects of the prior art, the present invention provides a preparation method and application of an excellent self-healing capacitor film and a capacitor thereof.

[0004] The technical solution of the present invention is as follows: A capacitor film with excellent self-healing properties, comprising a dielectric film, a functional layer being arranged on the surface of the dielectric film, the dielectric film being a BOPP film, i.e., a biaxially oriented polypropylene film, the functional layer being an aluminum oxide layer or a zinc oxide layer, and the material of the functional layer being a material having both a wide energy band gap and a high dielectric constant.

[0005] Preferably, the thickness of the functional layer is 100-200 nm.

[0006] A method for preparing a capacitor film with excellent self-healing properties comprises: vapor-depositing a functional layer on the surface of a dielectric film by vapor deposition to form a composite capacitor film with excellent self-healing properties.

[0007] Preferably, the dielectric film is further subjected to plasma treatment before evaporation.

[0008] Preferably, the method comprises the following steps: (1) BOPP film is plasma treated; (2) In the vacuum evaporation device, the functional layer raw material is heated by a resistance wire to vaporize it; (3) The BOPP film treated in step (1) is fed into the vacuum evaporation device in step (2), and the functional layer raw material vapor and oxygen form a functional layer film on the surface of the BOPP film; Completed the preparation of capacitor film with excellent self-healing properties.

[0009] Further preferably, the method for plasma treatment in step (1) is as follows: Ar gas is used as the working gas of the dielectric barrier discharge system, and the Ar gas enters the discharge region between the electrodes in the PECVD system at a flow rate of 4-8 L / min; two pieces of 0.5-2 mm thick glass are covered on the discharge electrodes as the dielectric barrier layer in the dielectric barrier discharge system; the discharge gap between the blocking dielectrics is 2-4 mm; the dielectric barrier discharge is driven by a microsecond pulse power supply; and a microsecond pulse voltage with an amplitude of 6.4-19.2 kV, a frequency of 1.2-1.8 kHz, a pulse width of 6-10 μs, and a rising edge of 400-600 ns is used as the discharge power supply.

[0010] More preferably, the Ar gas flow rate is 6 L / min, the glass thickness is 1 mm, the discharge gap is 2 mm, and the discharge power supply conditions are an amplitude of 12.8 kV, a frequency of 1.5 kHz, a pulse width of 8 μs, and a rising edge of 500 ns. Further preferably, in the step (2), the functional layer raw material is fed into an evaporation boat in a vacuum evaporation device as a metal source through a wire feeding system, and the evaporation boat is heated to a suitable temperature by passing an electric current through a resistance wire to vaporize the functional layer raw material.

[0011] Preferably, in step (2), a mixed gas of argon and oxygen is also introduced into the cavity of the vacuum evaporation device.

[0012] More preferably, in step (2), the flow ratio of argon to oxygen is maintained at (4-6):1, so that the functional layer raw material vapor reacts with oxygen to form a functional layer film. Argon is an inert gas that does not participate in the reaction. As a carrier gas, it can improve the uniformity of the dispersion of oxygen and the functional layer raw material vapor, thereby improving the uniformity of the obtained oxidized functional layer.

[0013] The excellent self-healing capacitor film or the high-temperature resistant capacitor film with excellent self-healing properties prepared by the preparation method is applied to the preparation of capacitors.

[0014] Further preferably, the preparation of the capacitor comprises the following steps: S1 Preparation of excellent self-healing capacitor film; S2 film slitting: cutting the capacitor film into the required size for winding; S3 core winding: winding the capacitor film onto the needle core to form the core of the film capacitor; S4 heat treatment: heating the capacitor core, removing impurities and shaping it; S5 gold spraying: spray a metal layer on both ends of the core to lead out the capacitor terminals; S6 Empowerment: Pressurize the capacitor core to improve its electrical performance; S7 potting: adding a shell to the outside of the capacitor core; Completed the preparation of high-temperature resistant metallized film capacitors with excellent self-healing properties.

[0015] Preferably, in step S4, the capacitor core is heat treated at 100° C. for 5-7 hours.

[0016] Preferably, in step S5, a zinc electrode is sprayed on the end surface of the core.

[0017] Preferably, in step S6, energization is performed by applying a 3000V DC voltage for 30s.

[0018] Preferably, in step S7, polyurethane is used to encapsulate the capacitor core.

[0019] The present invention has the following beneficial effects: 1. Aluminum oxide or zinc oxide with both high dielectric constant and high energy band gap is used as a functional layer deposited on the surface of BOPP film to suppress leakage current under high temperature and high field, and improve the high temperature electrical performance and self-healing characteristics of metallized film capacitors.

[0020] 2. The functional layer is constructed by plasma combined with evaporation. Compared with other deposition methods, this method has fewer film defects and better charge injection suppression effect. The functional layers deposited by evaporation, atomic layer deposition and magnetron sputtering all have more traps in the two ranges of 0.825eV~0.85eV and 0.9eV~0.925eV, and the trap depths are not much different. However, the high-temperature resistant capacitor film with excellent self-healing properties prepared by plasma combined with evaporation has a lower trap density, indicating that it has fewer defects. In addition, this method can match the production speed of capacitor films and is more suitable for industrial use.

[0021] 3. Use argon as the working gas during plasma pretreatment to improve the uniformity of the functional layer.

[0022] 4. Use plasma bombardment method to pre-treat the dielectric film to improve the adhesion of the functional layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Schematic diagram of BOPP film passing through plasma equipment; Figure 2Schematic diagram of equipment for evaporating aluminum oxide layer on BOPP film surface; Figure 3 Schematic diagram of the cross section of a capacitor core; Figure 4 Morphology of self-healing point of pure BOPP film; Figure 5 Morphology of the self-healing point of a high-temperature resistant capacitor film with excellent self-healing properties; Figure 6 Example 1 is a curve showing the change of the capacitance decay percentage of a capacitor over time at 70°C; Figure 7 Example 1 is a curve showing the change of the capacitance decay percentage of a capacitor over time at 85°C; Figure 8 Example 1 is a curve showing the change of the capacitance attenuation percentage of a capacitor over time at 90°C; Fig. 9 Example 1 is a curve showing the change of the capacitance decay percentage of a capacitor over time at 100°C; Fig.10 Example 1 is a curve showing the change of the capacitance attenuation percentage of the capacitor with the step voltage at 25°C; Fig.11 Example 1: Capacitance attenuation percentage curve of capacitor at 70°C as a function of step voltage; Fig.12 Example 1: Capacitance attenuation percentage curve of capacitor at 90°C as a function of step voltage; Fig.13 Example 1 is a curve showing the change of the capacitance attenuation percentage of the capacitor with the step voltage at 100°C; Fig.14 Comparative Example 1: Capacitance attenuation percentage curve of capacitor at 100°C versus time; Fig.15 Example 2 is a curve showing the change of the capacitance attenuation percentage over time at 100°C. Fig.16 Example 3 is a curve showing the change of the capacity attenuation percentage of the capacitor over time at 100°C. DETAILED DESCRIPTION

[0024] The present invention will be further described below in conjunction with embodiments and drawings.

[0025] Example 1 A capacitor film with excellent self-healing properties comprises a dielectric film, a functional layer is arranged on the surface of the dielectric film, the dielectric film is a BOPP film, the functional layer is an aluminum oxide layer, and the raw material of the functional layer is aluminum.

[0026] The method for preparing the capacitor film comprises the following steps: (1) BOPP film is subjected to plasma pretreatment; (2) In the vacuum evaporation device, the aluminum wire is heated by a resistance wire to vaporize it; (3) The BOPP film treated in step (1) is fed into the chamber of the vacuum evaporation device in step (2), and aluminum vapor and oxygen form an aluminum oxide functional layer on the surface of the BOPP film; Completed the preparation of excellent self-healing capacitor film.

[0027] Further preferably, in the step (1), the plasma pretreatment working gas is argon, and the argon enters the discharge region at a flow rate of 6 L / min; two pieces of 1 mm thick glass are covered on the discharge electrode as a dielectric barrier layer; the discharge gap between the blocking dielectrics is 2 mm; the dielectric barrier discharge is driven by a microsecond pulse power supply; and a microsecond pulse voltage with an amplitude of 12.8 kV, a frequency of 1.5 kHz, a pulse width of 8 μs, and a rising edge of 500 ns is used as the discharge power supply. Further preferably, in step (2), the aluminum wire is fed into the evaporation boat in the vacuum evaporation device as a metal source through the wire feeding system, and the evaporation boat is heated by the resistance wire to vaporize the aluminum; at the same time, a mixed gas of argon and oxygen is introduced into the cavity of the vacuum evaporation device, and the flow ratio of argon to oxygen is maintained at 5:1. The BOPP film (thickness of 8.8μm) is continuously fed into the vacuum chamber through the roller system, and the thickness of the aluminum oxide functional layer deposited on the surface can be adjusted by controlling the winding speed of the BOPP film, and the thickness is controlled at 150nm. The excellent self-healing capacitor film is used in the preparation of a capacitor, and the preparation of the capacitor includes the following steps: S1 Preparation of high temperature resistant capacitor film with excellent self-healing properties; S2 film slitting: cutting the capacitor film into the required size for winding; S3 core winding: Use 1350g winding tension and 1000g winding pressure to wind the capacitor film onto the needle core to form the core of the film capacitor; S4 heat treatment: heating the capacitor core at 100°C for 6 hours to remove impurities and set its shape; S5 gold spraying: Spray a 0.4mm thick gold layer on both ends of the core to lead out the capacitor terminals; S6 Energizing: Use 3000V DC voltage to pressurize the capacitor core for 30s to improve its electrical performance; S7 potting: Use polyurethane to encapsulate the capacitor core with a shell; Completed the preparation of high-temperature resistant metallized film capacitors with excellent self-healing properties.

[0028] In this embodiment, the width of the high temperature resistant metallized film capacitor with excellent self-healing properties is 75 mm, with a margin of 2.5 mm. The schematic diagram of the cross section of the capacitor core is as follows: Figure 3 As shown in the figure, the rated capacity of the capacitor is 70μF and the rated voltage is 2100VDC.

[0029] A wide energy bandgap can provide a high injection barrier at the electrode / dielectric interface, and a high dielectric constant can reduce the partial field strength on the functional layer, thereby inhibiting charge injection at the electrode / dielectric interface, reducing leakage current, improving voltage resistance, and reducing the probability of breakdown and self-healing when the capacitor is working at rated voltage. Therefore, the high-temperature electrical performance and self-healing characteristics of metallized film capacitors can be improved by depositing a functional layer with both a high dielectric constant and a high energy bandgap on the surface of the BOPP film.

[0030] The morphology of the functional layer was observed using SEM. The functional layer was relatively flat and had uniform thickness. The functional layer had good continuity and no obvious cracks, indicating that the plasma combined with evaporation method successfully constructed a relatively dense functional layer on the surface of the BOPP film.

[0031] The adhesion of the functional layer was evaluated. First, a 1m long capacitor film was placed flat on a rubber pad. Then, the 3M600 adhesion test tape was evenly pasted to the surface of the capacitor film with a length of 8cm. Finally, the torn part of the tape was perpendicular to the surface of the capacitor film and the tape was smoothly torn off. As a result, the functional layer did not fall off.

[0032] The method of the present invention can improve the high temperature electrical performance of the film capacitor mainly because it can effectively reduce its leakage current. The leakage current density of the pure BOPP film (the BOPP film not prepared in this embodiment) at 120°C and 500MV / m is 2.26×10 -4 A / m 2 , while the leakage current density of the composite film (the functional layer capacitor film deposited on the surface of the BOPP film prepared in this embodiment, hereinafter referred to as the composite film) is only 1.61×10 -4 A / m 2 , compared with the pure BOPP film, the leakage current density is reduced by about 29%. Due to the significantly reduced conduction loss, the composite film also shows a significantly higher breakdown field strength than the pure BOPP film. The breakdown field strength of the composite film reaches 720MV / m, which is 8% higher than the breakdown field strength of the pure BOPP film. The present invention uses metal needles to create artificial electrical weak points on the surfaces of different films, and uniformly applies a voltage of 3000V for 3s to cause the artificial electrical weak points to break down, and observes the area of ​​the self-healing points. Figure 4-5The morphology of the self-healing points of different metallized films observed by polarizing microscope is given. The self-healing point area of ​​the composite film is significantly smaller than that of the pure BOPP film, indicating that the presence of the aluminum oxide functional layer can effectively reduce the capacity decay. There may be two reasons for this: first, aluminum oxide has good thermal conductivity, and the heat generated during breakdown can be quickly dissipated through the electrode; second, the presence of the aluminum oxide functional layer reduces the self-healing energy of clearing the metal electrode and the BOPP film layer.

[0033] In actual operation, capacitors are usually continuously exposed to high field strengths, and the capacitor capacity gradually decays with the increase of pressurization time until failure. Therefore, the capacity decay percentage ((initial capacity - test capacity) / initial capacity) is an important indicator of the capacitor. Under room temperature conditions, a DC voltage of 2310VDC was applied to the capacitor sample for 24 hours for pretreatment, and the capacitance value after pressurization was recorded; under temperature conditions of 70℃, 85℃, 90℃, and 100℃, a DC voltage of 2940VDC was continuously applied to the capacitor sample, and the curves of the capacity decay percentage of different types of capacitors under different temperature conditions changing with time were obtained. The results are shown in Figure 2. Figure 6-9 . The capacity attenuation of pure BOPP film capacitors after pressurization for 440 hours at 70°C, 85°C, 90°C, and 100°C is 0.78%, 2.78%, 2.98%, and 7%, respectively. The functional layer can effectively reduce the capacity attenuation rate of film capacitors and improve the high-temperature DC durability of capacitors. GB / T 17702-2021 / IEC 61071:2017 requires that the capacitance value decrease after pressurization for 500 hours should not exceed 3% of the initial value. At 70°C and 85°C, the capacity attenuation of pure BOPP samples and composite film samples after pressurization for 500 hours is approximately 0.88%, 0.38%, 2.92%, and 1.51%, respectively, which can meet the requirements. However, at 90°C, after pressurization for 500 hours, the capacity attenuation of pure BOPP film reached 3.48%, which did not meet the requirements, while the capacity attenuation of composite film samples was 1.93%, which met the requirements. At 100°C, the capacity decay of the composite film is about 3%, which meets the requirements. Therefore, the surface construction of the functional layer increases the maximum operating temperature of the BOPP film capacitor by about 15°C.

[0034] Under different temperature conditions, different voltages were applied to the film capacitors for 300 seconds, and the capacity before and after the pressure was applied was tested. At 25°C, 70°C, 90°C and 100°C, the starting voltage of the composite film capacitor capacity decay was 500-1000V higher than that of the pure BOPP film capacitor. The results are shown in Figure 10-13 Since the composite film capacitor has a higher withstand voltage, the probability of self-healing breakdown is lower at the same voltage, and the starting voltage at which the capacitor capacity significantly decays is also higher. The higher the temperature, the greater the amplitude of the starting voltage.

[0035] In order to further study the different effects of each self-healing process on pure BOPP film capacitors and composite film capacitors, a step voltage with a starting value of 3150 VDC and a gradient of 200 VDC was applied to the capacitor. Each pressurization time was 10 s until the sample underwent 5 self-healing breakdowns. The capacity before and after 5 self-healing breakdowns was tested. The results are shown in Table 1.

[0036] Table 1 Capacitance changes of pure BOPP film capacitors and composite film capacitors after 5 self-healing

[0037] GB / T 17702-2021 / IEC 61071:2017 requires that the capacity change before and after five self-healing breakdowns should be less than ±0.5%. Pure BOPP film capacitors fail to meet the requirements, but composite film capacitors do.

[0038] After the composite film capacitor undergoes self-healing breakdown, only several layers of dielectric film adjacent to the initial breakdown point are melted, which has the characteristic of "isolation self-healing". After the pure BOPP film capacitor undergoes self-healing breakdown, dozens of layers of dielectric film are melted by the heat generated during self-healing.

[0039] Comparative Example 1 Based on Example 1, the capacitor film preparation did not undergo the plasma pretreatment in step (1), but only underwent treatments (2) to (3). Other steps were the same as in Example 1. The results are shown in FIG. Fig.14 .

[0040] By comparing Example 1 with Comparative Example 1, it can be seen that the effect of combining plasma with evaporation is the best. This may be because after plasma bombardment, certain defects may be formed on the pure BOPP film, which is conducive to the extension of aluminum oxide on the defects into the BOPP film, providing the adsorption performance of the composite film and improving the self-healing ability of the capacitor at high temperature during long-term use.

[0041] Example 2 Based on Example 1, the working gas for the capacitor film preparation step (1) plasma pretreatment is air, and the results are shown in Fig.15 .

[0042] It can be seen from Examples 1 and 2 that argon is the best working gas for plasma bombardment, while air is slightly less effective. This may be because argon is easier to ionize than air, producing more plasma, which enhances the bonding strength between the BOPP film and the functional layer, making the composite film have excellent self-healing properties.

[0043] Example 3 Based on Example 1, the material of the functional layer was changed to zinc oxide, and the other parts were the same as Example 1. The results are shown in Fig.16 .

[0044] It can be seen from Examples 1 and 3 that the effect of aluminum oxide is better than that of zinc oxide. This may be because aluminum oxide has both a better energy band gap and a dielectric constant. At the same time, aluminum oxide is tightly adsorbed to the BOPP film, so that the composite film has excellent self-healing properties. The above embodiments are only preferred technical solutions of the present invention and should not be regarded as limitations of the present invention. The embodiments and features in the embodiments of the present application can be arbitrarily combined with each other without conflict. The protection scope of the present invention shall be the technical solutions recorded in the claims, including the equivalent replacement solutions of the technical features in the technical solutions recorded in the claims. That is, equivalent replacement improvements within this scope are also within the protection scope of the present invention.

Claims

1. A capacitor film having excellent self-healing properties, characterized in that: The capacitor film comprises a dielectric film, a functional layer is arranged on the surface of the dielectric film, the dielectric film is a BOPP film, and the material of the functional layer is a material having both a wide energy band gap and a high dielectric constant. The functional layer is an aluminum oxide layer or a zinc oxide layer.

2. A method for preparing a high temperature resistant capacitor film with excellent self-healing properties, characterized in that: The method is to evaporate a functional layer on the surface of a dielectric film by evaporation to form a capacitor film with excellent self-healing properties.

3. The method for preparing a high temperature resistant capacitor film with excellent self-healing properties according to claim 2, characterized in that: The dielectric film is also subjected to plasma treatment before evaporation.

4. The method for preparing the excellent self-healing capacitor film according to claim 2 or 3, characterized in that: The functional layer material is aluminum or zinc.

5. The method for preparing the excellent self-healing capacitor film according to claim 4, characterized in that: The method comprises the following steps: (1) BOPP film is subjected to plasma pretreatment; (2) In the vacuum evaporation device, the functional layer raw material is heated by a resistance wire to vaporize it; (3) The BOPP film treated in step (1) is fed into the vacuum evaporation device in step (2), and the functional layer raw material vapor and oxygen form a functional layer film on the surface of the BOPP film; Completed the preparation of capacitor film with excellent self-healing properties.

6. The method for preparing a capacitor film having excellent self-healing properties according to claim 5, characterized in that: The method of plasma pretreatment in step (1) is: argon or air is used as the plasma pretreatment working gas.

7. The method for preparing a capacitor film having excellent self-healing properties according to claim 6, characterized in that: The plasma pretreatment working gas enters the discharge area at a flow rate of 4-8L / min; two pieces of 0.5-2mm thick glass are covered on the discharge electrode as a dielectric barrier layer; the discharge gap between the blocking dielectrics is 2-4mm; the dielectric barrier discharge is driven by a microsecond pulse power supply; a microsecond pulse voltage with an amplitude of 6.4-19.2kV, a frequency of 1.2-1.8kHz, a pulse width of 6-10μs, and a rising edge of 400-600ns is used as the discharge power supply; preferably, the plasma pretreatment working gas is argon, the argon gas flow rate is 6L / min, the glass thickness is 1mm, and the discharge gap is 2mm; the discharge power supply conditions are an amplitude of 12.8kV, a frequency of 1.5kHz, a pulse width of 8μs, and a rising edge of 500ns.

8. The method for preparing a capacitor film having excellent self-healing properties according to claim 5, characterized in that: In the step (2), a mixed gas of argon and oxygen is introduced into the cavity of the vacuum evaporation device.

9. The method for preparing a capacitor film having excellent self-healing properties according to claim 8, characterized in that: The flow ratio of argon to oxygen is (4-6):1, so that the functional layer raw material steam reacts with oxygen to form a functional layer; preferably, the flow ratio of argon to oxygen is 5:

1.

10. The excellent self-healing capacitor film according to claim 1 or the high temperature resistant capacitor film with excellent self-healing properties prepared by the preparation method according to any one of claims 2 to 9 is used in the preparation of capacitors.

Citation Information

Cited By

  • An Adaptive Control Method for Plasma Processing of BOPP Thin Films

    CN122945506B