Semiconductor nanowire, preparation method thereof and application of semiconductor nanowire in lithium ion battery
By growing semiconductor nanowires on the surface of metal current collector/carbon materials of waste lithium-ion batteries, the problems of high cost and poor performance in lithium-ion battery recycling and silicon negative electrode material preparation are solved, and the recycling of high-performance battery materials is realized and Environmentally friendly battery performance improvement.
Patent Information
- Application Number
- CN202411064613.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
In the recycling process of existing lithium-ion batteries, especially the preparation method of silicon negative electrode materials, there are problems such as high cost, poor performance and complex processes, and the recycling of harmful substances in waste lithium batteries is difficult to achieve, resulting in environmental pollution and waste of resources.
Magnetically controlled sputtering technology is used to prepare metal tin films on the surface of metal current collector/carbon materials of waste lithium-ion batteries, and semiconductor nanowires are grown through chemical vapor deposition technology, simplifying the process, improving conductivity and electrochemical performance, directly on carbon materials Semiconductor nanowires are grown on the surface to improve battery performance.
It realizes high-performance recycling of waste lithium-ion battery materials, reduces environmental pollution, improves the battery's charging and discharge cycle stability and service life, and reduces production costs.
Smart Images

Figure CN118957532A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a semiconductor nanowire and a preparation method thereof and application in lithium ion batteries. Background Art
[0002] With the popularity of electric vehicles and portable electronic products, the number of discarded lithium batteries has increased dramatically. Since discarded batteries contain harmful substances, they pose a threat to the environment. If they cannot be recycled, they will also lead to a serious waste of secondary metal resources.
[0003] In the recycling process of waste lithium-ion batteries, copper foil is usually used as the negative electrode current collector, and carbon materials are usually used as the negative electrode active material. The recycling of copper foil and carbon materials is crucial for resource recycling and reducing environmental pollution. Several methods may be used in the recycling process of copper foil / carbon film negative electrodes: mechanical separation, hydrometallurgy, thermal metallurgy, etc. For carbon film, it is usually used as the active material of the battery negative electrode, and its recycling is very complicated. The recycling of carbon materials can be peeled off from the electrode by chemical or thermal treatment methods, and further processing is required before it can be used again in battery manufacturing. The entire recycling process is very complicated, while also ensuring the safety of the operation and environmental sustainability.
[0004] Silicon negative electrode lithium battery is a lithium-ion battery with silicon as negative electrode material. At present, the main preparation methods of silicon negative electrode are chemical vapor deposition, sol-gel method and pyrolysis method. Among them, chemical vapor deposition method has simple process and high yield, but high cost; sol-gel method has the advantages of simple process and low cost, but the carbon silicon negative electrode prepared has uneven structure and poor cycle performance; pyrolysis method also has the advantages of simple process and low cost, but the carbon silicon negative electrode prepared has rough structure and poor conductivity. In addition, the current silicon negative electrode also has the problems of volume expansion and interface impedance.
[0005] Based on the above, a new method for recycling discarded lithium-ion batteries is needed, and combined with silicon negative electrodes, the waste battery materials can be converted into high-performance electrode materials. Summary of the invention
[0006] 1. Technical issues to be resolved
[0007] In view of the deficiencies in the prior art, the present invention provides a semiconductor nanowire and a method for preparing the same and an application in a lithium-ion battery, which solves the problems raised in the above-mentioned background technology.
[0008] (II) Technical solution
[0009] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0010] According to a first aspect of the present invention, there is provided a method for preparing a semiconductor nanowire, comprising the following steps:
[0011] A metal tin film is prepared on a substrate by using a magnetron sputtering technique, and then semiconductor nanowires are prepared on the surface of the metal tin film by using a chemical vapor deposition technique;
[0012] Wherein, the substrate is selected from metal current collector / carbon material of waste lithium-ion batteries.
[0013] Preferably, the parameters for preparing the metal tin film on the substrate using magnetron sputtering technology are: introducing argon gas at room temperature and 1.0-10 Pa, and coating for 1-30 minutes to obtain the metal tin film, wherein the plasma power of the magnetron sputtering is 10-100W, and the flow rate of the argon gas is 50-200sccm.
[0014] Preferably, the parameters for preparing semiconductor nanowires on the surface of the metal tin film by chemical vapor deposition technology are: under the conditions of 235-300°C and 80-1000Pa, a mixed gas containing hydrogen, silane, germane and phosphine is introduced, and the silicon germanium nanowires are grown for 5-180 minutes, wherein the plasma power of the chemical vapor deposition is 5-100W, and the flow rate of the mixed gas is 50-200sccm.
[0015] Preferably, the flow ratio of hydrogen, silane, germane and phosphine in the mixed gas is 200: 0.1-5: 0.01-0.1: 0.01-0.1.
[0016] Preferably, the parameters for preparing semiconductor nanowires on the surface of the metal tin film by chemical vapor deposition technology are: under the conditions of 235-300°C and 80-1000Pa, a mixed gas containing hydrogen, silane and phosphine is introduced, and the silicon nanowires are grown for 5-180 minutes, wherein the plasma power of the chemical vapor deposition is 5-100W, and the flow rate of the mixed gas is 50-200sccm.
[0017] Preferably, the flow ratio of hydrogen, silane and phosphine in the mixed gas is 200:0.1-5:0.01-0.1.
[0018] Preferably, the metal tin film is subjected to reduction treatment before preparing semiconductor nanowires on the surface of the metal tin film, and the parameters of the reduction treatment are: at 100-350°C, 80-500Pa, introducing 100-500sccm of hydrogen and treating at a plasma power of 5-200W for 2-60min.
[0019] According to a second aspect of the present invention, there is provided a semiconductor nanowire obtained according to the above preparation method.
[0020] According to a third aspect of the present invention, there is provided a use of a semiconductor nanowire as a negative electrode of a lithium ion battery in a lithium ion battery.
[0021] (III) Beneficial effects
[0022] The present invention provides a semiconductor nanowire and a preparation method thereof and application in a lithium-ion battery. The invention has the following beneficial effects:
[0023] (1) This solution provides a method for preparing semiconductor nanowires, which uses metal current collectors / carbon materials from waste lithium-ion batteries, and directly prepares semiconductor nanowires on the surface of carbon materials without any recycling. The prepared semiconductor nanowires have excellent electrical conductivity and electrochemical properties, and growing semiconductor nanowires on the surface of carbon materials from waste lithium-ion batteries can further improve the performance of the battery.
[0024] (2) The present invention provides a method for preparing semiconductor nanowires, which can prevent the carbon film from falling off the copper foil and becoming powderized by regulating the chemical vapor deposition conditions of the semiconductor nanowires.
[0025] (3) The method for preparing semiconductor nanowires provided in this solution realizes the recycling of waste lithium-ion battery materials and reduces environmental pollution. In addition, the prepared semiconductor nanowires have uniform morphology and size, and can be used as negative electrode materials in lithium-ion batteries to improve the battery's charge and discharge cycle stability and extend the battery's service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a scanning electron microscope image of silicon germanium nanowires prepared in Example 1 of the present invention;
[0027] Figure 2 This is an X-ray energy dispersion spectrum analysis diagram of silicon germanium nanowires prepared in Example 1 of the present invention;
[0028] Figure 3 This is a scanning electron microscope image of silicon nanowires prepared in Example 2 of the present invention;
[0029] Figure 4 This is a scanning electron microscope image of the carbon film of the waste lithium-ion battery used in the present invention;
[0030] Figure 5 The discharge capacity and coulombic efficiency of the materials obtained in Example 1, Example 2 and Comparative Example 1 of the present invention as negative electrode materials in 120 cycles. DETAILED DESCRIPTION
[0031] In order to better illustrate the content of the present invention, a detailed description is given below in conjunction with specific embodiments.
[0032] The present invention provides a method for preparing semiconductor nanowires, comprising the following steps:
[0033] A metal tin film is prepared on a substrate by using a magnetron sputtering technique, and then semiconductor nanowires are prepared on the surface of the metal tin film by using a chemical vapor deposition technique;
[0034] Wherein, the substrate is selected from metal current collector / carbon material of waste lithium-ion batteries.
[0035] It should be noted that before growing the semiconductor nanowires, a layer of metal tin film is first deposited to catalyze the subsequent growth of the semiconductor nanowires.
[0036] The present invention directly grows semiconductor nanowires on the surface of the metal current collector / carbon material of the waste lithium ion battery, which not only improves the recycling rate of the waste battery materials, but also simplifies the preparation process of traditional lithium ion battery materials, reduces production costs and improves battery performance by directly growing semiconductor nanowires on the surface of the carbon material of the waste lithium ion battery.
[0037] In a specific embodiment, the parameters for preparing a metal tin film on a substrate using magnetron sputtering technology are: introducing argon gas at room temperature and 1.0-10Pa, and coating for 1-30min to obtain a metal tin film, wherein the plasma power of magnetron sputtering is 10-100W, and the flow rate of argon gas is 50-200sccm. Preferably, the parameters for preparing a metal tin film are: introducing argon gas at room temperature and 2.5Pa, introducing argon gas at a flow rate of 100sccm, and preparing a metal tin film on the surface of a carbon material at a plasma power of 20W. By controlling the parameters of magnetron sputtering, a metal tin film with better adhesion and uniformity can be obtained, providing a stable platform for growing semiconductor nanowires.
[0038] The semiconductor nanowires of the present invention are silicon germanium nanowires or silicon nanowires. When preparing silicon germanium nanowires, the corresponding preparation parameters are:
[0039] At 235-300°C and 80-1000Pa, a mixed gas containing hydrogen, silane, germane and phosphine is introduced, and the growth is 5-180min to obtain silicon germanium nanowires, wherein the plasma power of chemical vapor deposition is 5-100W, and the flow rate of the mixed gas is 50-200sccm. Preferably, the parameters for preparing silicon germanium nanowires are: at 250°C and 700Pa, the following mixed gas is introduced: 195sccm of hydrogen; 1sccm of silane; 15sccm of germane (1% concentration in hydrogen); 2sccm of phosphine (1% concentration in hydrogen), and the silicon germanium nanowires are grown for 30min at a plasma power of 15W. By controlling the specific parameters of chemical vapor deposition, the composition and structure of silicon germanium nanowires can be precisely controlled. In addition, under low temperature conditions, the carbon material can be effectively prevented from falling off the copper foil and pulverizing.
[0040] When preparing silicon nanowires, the mixed gas includes only hydrogen, silane and phosphine, and does not contain germane.
[0041] In a specific embodiment, the metal tin film is subjected to a reduction treatment before preparing the semiconductor nanowires. The reduction treatment can enhance the catalytic effect of the metal tin film on the process of growing silicon germanium nanowires, and further enhance the chemical stability and cycle performance of the semiconductor nanowires.
[0042] The following is a further description of a method for preparing semiconductor nanowires provided by the present invention in conjunction with specific embodiments.
[0043] Example 1
[0044] Step 1, preparing a metal tin film: placing the metal current collector / carbon material substrate of the waste lithium-ion battery in a magnetron sputtering chamber, introducing 100 sccm of argon gas at room temperature and 2.5 Pa, controlling the plasma power to be 20 W, coating the carbon material surface for 6 minutes, and obtaining a metal tin film;
[0045] Step 2, hydrogen reduction: the substrate is placed in the PECVD chamber, the temperature in the chamber is adjusted to 250°C, 130Pa, hydrogen is introduced at a flow rate of 100 sccm, and the treatment is carried out at a plasma power of 5W for 10 minutes to reduce the tin oxide on the metal tin film;
[0046] Step 3, preparation of silicon germanium nanowires: maintaining the temperature in the PECVD chamber at 250°C, under the condition of 130Pa, introducing 195sccm of hydrogen; 1sccm of silane; 15sccm of germane (1% concentration in hydrogen); 2sccm of phosphine (1% concentration in hydrogen), and growing for 30min at a plasma power of 15W to prepare silicon germanium nanowires.
[0047] The surface morphology of the silicon germanium nanowires prepared in this embodiment was analyzed. Figure 1 and Figure 2 As shown, according to Figure 1 It can be seen that the silicon germanium nanowires prepared in this embodiment have uniform morphology and size. Figure 2 It can be seen that the prepared silicon germanium nanowires contain Si, Ge and Sn elements, and the Si, Ge and Sn elements are evenly distributed, which can effectively improve the battery discharge capacity and cycle efficiency.
[0048] Example 2
[0049] The preparation method of this embodiment is the same as that of embodiment 1, except that the mixed gas in step 3 does not contain germanium, and the silicon nanowires are prepared. Figure 3 shown.
[0050] Comparative Example 1
[0051] This comparative example is directly selected from the metal current collector / carbon material of the waste lithium ion battery without growing silicon germanium nanowires on the surface of the carbon material, such as Figure 4 shown.
[0052] Application Examples
[0053] The samples of Example 1, Example 2 and Comparative Example 1 were respectively prepared into half-cell lithium batteries, wherein the electrolyte of the lithium battery was selected from lithium iron phosphate, the positive electrode was a lithium sheet, and the active material was charged and discharged at a current of 200 mA / g, and the discharge capacity and coulomb efficiency after 120 cycles were tested. Figure 5 As shown, from Figure 5 It can be seen that after 120 cycles, the mass specific capacity of the carbon film is only 250mA / g. The mass specific capacity of the silicon germanium nanowires prepared in Example 1 is maintained at 2000mA / g, which is 8 times that of the carbon film. The mass specific capacity of the silicon nanowires in Example 2 is maintained at 900mA / g, which is also significantly better than the carbon film.
[0054] By applying the prepared semiconductor nanowires to lithium-ion batteries, it can be found that the semiconductor nanowires prepared by the present invention not only have high specific capacity and cycle life, but also can realize the reuse of metal current collectors / carbon materials of waste lithium-ion batteries, save energy and reduce environmental pollution.
[0055] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing semiconductor nanowires, characterized in that: The following steps are involved: A metal tin film is prepared on a substrate by using a magnetron sputtering technique, and then semiconductor nanowires are prepared on the surface of the metal tin film by using a chemical vapor deposition technique; Wherein, the substrate is selected from metal current collector / carbon material of waste lithium-ion batteries.
2. The method for preparing semiconductor nanowires according to claim 1, characterized in that: The parameters for preparing the metal tin film on the substrate using the magnetron sputtering technology are: introducing argon gas at room temperature and 1.0-10Pa, and coating for 1-30 minutes to obtain the metal tin film, wherein the plasma power of the magnetron sputtering is 10-100W, and the flow rate of the argon gas is 50-200sccm.
3. The method for preparing semiconductor nanowires according to claim 1, characterized in that: The parameters for preparing semiconductor nanowires on the surface of the metal tin film by chemical vapor deposition technology are: under the conditions of 235-300°C and 80-1000Pa, a mixed gas containing hydrogen, silane, germane and phosphine is introduced to grow for 5-180 minutes to obtain silicon germanium nanowires, wherein the plasma power of chemical vapor deposition is 5-100W, and the flow rate of the mixed gas is 50-200sccm.
4. The method for preparing semiconductor nanowires according to claim 3, characterized in that: The flow ratio of hydrogen, silane, germane and phosphine in the mixed gas is 200: 0.1-5: 0.01-0.1: 0.01-0.
1.
5. The method for preparing semiconductor nanowires according to claim 1, characterized in that: The parameters for preparing semiconductor nanowires on the surface of the metal tin film by chemical vapor deposition technology are: under the conditions of 235-300°C and 80-1000Pa, a mixed gas containing hydrogen, silane and phosphine is introduced, and the silicon nanowires are grown for 5-180 minutes, wherein the plasma power of the chemical vapor deposition is 5-100W, and the flow rate of the mixed gas is 50-200sccm.
6. The method for preparing semiconductor nanowires according to claim 5, characterized in that: The flow ratio of hydrogen, silane and phosphine in the mixed gas is 200:0.1-5:0.01-0.
1.
7. The method for preparing semiconductor nanowires according to claim 1, characterized in that: Before preparing semiconductor nanowires on the surface of the metal tin film, the metal tin film is subjected to reduction treatment, and the parameters of the reduction treatment are: at 100-350° C., 80-500 Pa, 100-500 sccm of hydrogen is introduced and the treatment is carried out at a plasma power of 5-200 W for 2-60 minutes.
8. A semiconductor nanowire obtained according to the preparation method according to any one of claims 1 to 7.
9. Use of the semiconductor nanowire according to claim 8 as a negative electrode of a lithium ion battery in a lithium ion battery.
Citation Information
Cited By
Silicon nanowire and preparation method and application thereof
CN120527378A
Silicon nanowire and its preparation method and application
CN120527378B