Hydrogen evolution catalyst for electrolyzed water and preparation method thereof
By growing cobalt-copper bimetallic hydroxide on nickel foam and coating it with graphylene, a ternary composite catalyst was formed, which solved the problems of insufficient durability and electrocatalytic activity of non-precious metal catalysts under high current density and realized a highly efficient water electrolysis hydrogen production technology.
Patent Information
- Application Number
- CN202411180296.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
AI Technical Summary
Existing non-precious metal hydrogen evolution catalysts for water electrolysis lack durability and electrocatalytic activity at high current densities, and are sensitive to pH and temperature, which limits the commercialization of water electrolysis technology.
A ternary composite catalyst was prepared by growing cobalt-copper bimetallic hydroxide on the inner and outer surfaces of the pores of a nickel foam sheet and coating it with graphyne. The catalyst was prepared using a specific molar ratio of soluble cobalt and copper salts.
It significantly improves the durability and electrocatalytic activity of hydrogen evolution catalysts for water electrolysis at high current densities, reduces overpotential, and is suitable for large-scale production and commercial applications.
Smart Images

Figure CN118957667A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrocatalysis, and in particular to a hydrogen evolution catalyst for water electrolysis and a preparation method thereof. Background Art
[0002] With the continuous growth of global energy demand and the increasingly severe environmental problems, the development of efficient and economical electrochemical energy conversion technology has become a research hotspot. Among them, hydrogen production by water electrolysis has received widespread attention as a clean energy conversion method. Traditional water electrolysis technology mainly relies on precious metal materials (such as platinum) as catalysts for the hydrogen evolution reaction (HER) (i.e., hydrogen evolution catalysts), but the high cost and resource scarcity of precious metal materials limit their large-scale application. Therefore, the development of non-precious metal materials that can still maintain high performance at high current density as hydrogen evolution catalysts is of great significance to promote the commercialization of water electrolysis technology.
[0003] In the past few decades, a variety of non-precious metal materials have been studied as hydrogen evolution catalysts. These non-precious metal materials include transition metal compounds, metal organic frameworks (MOFs), carbon materials and their composites. These non-precious metal materials reduce the manufacturing cost, but their durability and electrocatalytic activity at high current density remain a challenge. High current density means higher energy conversion efficiency, but it also puts higher requirements on the durability and electrocatalytic activity of hydrogen evolution catalysts.
[0004] For example, in the prior art, iron-cobalt double hydroxide is usually used as a hydrogen evolution catalyst, but its overpotential is still higher (i.e., the electrocatalytic activity is lower) compared with precious metal materials. In addition, iron-based materials are highly sensitive to pH and temperature and will be corroded under certain electrolyte conditions, which adversely affects their service life.
[0005] Therefore, it is necessary to develop a new type of hydrogen evolution catalyst for water electrolysis, which can have excellent durability and electrocatalytic activity at high current density. Summary of the invention
[0006] Technical issues
[0007] The first object of the present invention is to provide a method for preparing a hydrogen evolution catalyst for water electrolysis, which has a simple process, can be carried out at low cost, and can achieve large-scale production.
[0008] The second object of the present invention is to provide a novel hydrogen evolution catalyst for water electrolysis prepared by the above method, which can be used at a high current density (e.g., 50 to 100 mA·cm -2) has excellent durability and electrocatalytic activity under low temperature. Specifically, the hydrogen evolution catalyst for water electrolysis can be used as a catalyst for the hydrogen evolution reaction (HER) occurring at the cathode of the electrolyzer. Excellent electrocatalytic activity means that, compared with conventional hydrogen evolution catalysts, the overpotential of the hydrogen evolution catalyst of the present invention measured by the linear sweep voltammetry curve is significantly reduced.
[0009] Technical Solution
[0010] According to a first aspect of the present invention, there is provided a method for preparing a hydrogen evolution catalyst for water electrolysis, the method comprising the following steps:
[0011] (a) preparing a nickel foam sheet, and cleaning the nickel foam sheet to remove surface impurities;
[0012] (b) dissolving a stabilizer, a reaction aid, a soluble cobalt salt and a soluble copper salt in a first solvent to obtain a first solution, and placing the pretreated nickel foam sheet in the first solution, wherein the molar ratio of the soluble cobalt salt to the soluble copper salt is 1:5 to 1:7,
[0013] Then, a hydrothermal reaction is performed to grow cobalt-copper double metal hydroxide on the inner and outer surfaces of the pores of the pretreated nickel foam sheet.
[0014] The obtained product is then washed to obtain an intermediate;
[0015] (c) preparing a mixture comprising a second solvent and hexa(trimethylsilylethynyl)benzene as a graphyne precursor, and adding a diluent and a buffer to obtain a second solution, and adding Cu foil and the intermediate to the second solution,
[0016] Then, a heating reaction is carried out under an inert atmosphere to grow graphene on the intermediate.
[0017] Then, the obtained product is washed and dried to obtain the hydrogen evolution catalyst for water electrolysis.
[0018] In one embodiment, in step (a),
[0019] The prepared nickel foam sheet has a length of 1 to 1.5 cm, a width of 1 to 1.5 cm, a thickness of 0.03 to 0.05 cm, and
[0020] In the cleaning, the nickel foam sheet is ultrasonically treated with HCl solution, alcohol solvent and water in sequence.
[0021] The alcohol solvent is at least one of ethanol and ethylene glycol,
[0022] The water is at least one of deionized water, ion exchange water, distilled water and ultrapure water.
[0023] In one embodiment, in step (b),
[0024] In the first solution, the stabilizer is at least one of urea, urea, and ethylenediamine.
[0025] The reaction aid is at least one of ammonium fluoride and ammonium chloride,
[0026] The soluble cobalt salt is at least one of cobalt nitrate, cobalt sulfate and cobalt chloride.
[0027] The soluble copper salt is at least one of copper nitrate, copper sulfate and copper chloride.
[0028] The first solvent is at least one of ultrapure water, deionized water, ethanol and acetone.
[0029] In one embodiment, in step (b),
[0030] Relative to 1g pretreated nickel foam sheet,
[0031] The amount of the stabilizer is 0.01 to 0.1 g.
[0032] The dosage of the reaction aid is 0.01 to 0.1 g.
[0033] The total amount of the soluble cobalt salt and the soluble copper salt is 1 to 2 mmol,
[0034] The volume of the first solvent is 20-50 ml.
[0035] In one embodiment, in step (b),
[0036] The temperature of the hydrothermal reaction is 80-160°C.
[0037] The hydrothermal reaction time is 4 to 12 hours.
[0038] The cleaning is performed by using an organic cleaning agent and water in sequence.
[0039] In one embodiment, in step (c),
[0040] The second solvent is pyridine or a pyridine derivative, wherein the pyridine derivative is at least one selected from bipyridine, polyvinyl pyridine, and polymer-bonded 4-(dimethylamino)-pyridine.
[0041] The diluent is at least one of acetone, methanol, ethanol, ethylene glycol, isopropanol, N,N-dimethylformamide, carbon tetrachloride, dimethyl sulfoxide, and ultrapure water.
[0042] The buffer is at least one of tetramethylethylenediamine, bicarbonate buffer, and acetic acid / sodium acetate buffer.
[0043] In one embodiment, in step (c),
[0044] Relative to 1g pretreated nickel foam sheet,
[0045] The dosage of the second solvent is 50-100 ml.
[0046] The amount of hexa(trimethylsilylethynyl)benzene used is 0.05-0.1 mmol, and it is used by dissolving in the second solvent.
[0047] The volume ratio of the diluent to the buffer is 50:1 to 200:1,
[0048] The usage amount of the diluent is 50 to 120 ml.
[0049] The amount of the Cu foil is 0.5-2 g.
[0050] In one embodiment, in step (c),
[0051] The inert atmosphere is at least one of an argon atmosphere and a nitrogen atmosphere.
[0052] The temperature of the heating reaction is 40-60°C,
[0053] The heating reaction time is 20 to 48 hours.
[0054] The cleaning is performed by using an organic cleaning agent and water in sequence.
[0055] The drying is vacuum drying, the drying temperature is 40 to 60° C., and the drying time is 8 to 24 hours.
[0056] According to a second aspect of the present invention, there is provided a hydrogen evolution catalyst for water electrolysis, which is prepared by the above method, wherein the hydrogen evolution catalyst comprises a nickel foam sheet, a cobalt-copper double metal hydroxide and graphyne,
[0057] Wherein, the cobalt-copper double metal hydroxide is located on the inner and outer surfaces of the pores of the nickel foam sheet.
[0058] The graphyne is located on the cobalt-copper double hydroxide, and
[0059] The pores in the hydrogen evolution catalyst correspond to the pores in the nickel foam sheet.
[0060] In one embodiment, the hydrogen evolution catalyst is used as a cathode of an electrolyzer while serving as a catalyst for the hydrogen evolution reaction.
[0061] Beneficial Effects
[0062] Compared with the prior art, the method of the present invention grows cobalt-copper double hydroxide on the inner and outer surfaces of the pores of the nickel foam sheet (i.e., all surfaces of the nickel foam sheet), and then grows graphyne on the cobalt-copper double hydroxide, thereby preparing a hydrogen evolution catalyst for water electrolysis.
[0063] In particular, the present invention prepares a cobalt-copper double metal hydroxide by using a soluble cobalt salt and a soluble copper salt having a specific molar ratio, thereby significantly improving the durability and electrocatalytic activity of a hydrogen evolution catalyst for water electrolysis at a high current density.
[0064] The method of the invention has simple process and high cost-effectiveness, and provides feasibility for large-scale promotion of hydrogen production technology by electrolysis of water.
[0065] In addition, the hydrogen evolution catalyst for water electrolysis of the present invention is a ternary composite material, in a sheet shape, and has pores corresponding to the original pores in the nickel foam sheet. The nickel foam sheet is used as a substrate, the cobalt copper double metal hydroxide is used as an active component of the catalyst, and the graphyne is used as a protective agent for the cobalt copper double metal hydroxide.
[0066] The hydrogen evolution catalyst significantly increases the specific surface area of the cobalt-copper double metal hydroxide by maintaining the porous characteristics of the nickel foam sheet substrate, thereby providing more active sites for the hydrogen evolution reaction (HER), thereby improving the electrocatalytic efficiency.
[0067] Furthermore, graphyne is used to effectively enhance the chemical and mechanical stability of cobalt-copper double hydroxide while maintaining its excellent electrocatalytic activity. Moreover, graphyne also promotes rapid charge transfer through its unique electronic structure.
[0068] The invention can make the obtained hydrogen evolution catalyst for water electrolysis have excellent durability and electrocatalytic activity under high current density through the synergistic effect of the nickel foam sheet, the cobalt-copper double metal hydroxide and the graphyne.
[0069] In addition, the hydrogen evolution catalyst for water electrolysis of the present invention exhibits good performance consistency and repeatability in practical applications and is suitable for large-scale production and commercial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] Figure 1 3 is a scanning electron microscope photograph of the hydrogen evolution catalyst for water electrolysis obtained according to Comparative Example 1 of the present invention.
[0071] Figure 2 1 is a scanning electron microscope photograph of the hydrogen evolution catalyst for water electrolysis obtained according to Example 1 of the present invention. DETAILED DESCRIPTION
[0072] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings.
[0073] Unless otherwise defined, all terms used herein, including technical or scientific terms, should be interpreted as having the same meaning as commonly understood by ordinary technicians in the field to which the present invention belongs. Therefore, unless explicitly defined, terms such as those defined in commonly used dictionaries should not be interpreted in an ideal or overly formal sense.
[0074] When the conditions and methods for measuring a property or parameter described in this specification are not described in detail, the property or parameter can be measured using the measurement conditions and methods generally used by those skilled in the art.
[0075] Unless otherwise specified, "%" used herein means % by weight.
[0076] 1. Method for preparing hydrogen evolution catalyst for water electrolysis
[0077] According to a first aspect of the present invention, there is provided a method for preparing a hydrogen evolution catalyst for water electrolysis, the method comprising the following steps:
[0078] (a) preparing a nickel foam sheet, and cleaning the nickel foam sheet to remove surface impurities;
[0079] (b) dissolving a stabilizer, a reaction aid, a soluble cobalt salt and a soluble copper salt in a first solvent to obtain a first solution, and placing the pretreated nickel foam sheet in the first solution, wherein the molar ratio of the soluble cobalt salt to the soluble copper salt is 1:5 to 1:7,
[0080] Then, a hydrothermal reaction is performed to grow cobalt-copper double metal hydroxide on the inner and outer surfaces of the pores of the pretreated nickel foam sheet.
[0081] The obtained product is then washed to obtain an intermediate;
[0082] (c) preparing a mixture comprising a second solvent and hexa(trimethylsilylethynyl)benzene as a graphyne precursor, and adding a diluent and a buffer to obtain a second solution, and adding Cu foil and the intermediate to the second solution,
[0083] Then, a heating reaction is carried out under an inert atmosphere to grow graphene on the intermediate.
[0084] Then, the obtained product is washed and dried to obtain the hydrogen evolution catalyst for water electrolysis.
[0085] Hereinafter, the preparation method of the present invention will be described in detail with respect to each step.
[0086] Step (a) Pretreatment
[0087] A nickel foam sheet is prepared, and the nickel foam sheet is cleaned to remove surface impurities.
[0088] The nickel foam sheet can be prepared by conventional processes. For example, by cutting the commercially available original nickel foam material into suitable sizes, such as 1 to 1.5 cm in length, 1 to 1.5 cm in width, and 0.03 to 0.05 cm in thickness, a nickel foam sheet used as a reaction substrate can be obtained. The nickel foam sheet is in the form of a thin sheet, and has a large number of interconnected pores inside, so it has a high porosity and specific surface area. The cobalt-copper double metal hydroxide grown on its surface will also have a high specific surface area, thereby providing more reaction sites.
[0089] Then, the nickel foam sheet can be cleaned by conventional processes to remove surface impurities. For example, the nickel foam sheet can be soaked in three cleaning agents, namely, HCl solution, alcohol solvent, and ultrapure water, in sequence, and then subjected to ultrasonic treatment.
[0090] The HCl solution is mainly used to remove inorganic impurities (such as oxides and dirt) on the surface of the nickel foam sheet. The concentration of the HCl solution can be 3-6M.
[0091] If the concentration is higher than 6M, the structure of the nickel foam may be destroyed, affecting the structure and specific surface area of the cobalt-copper double hydroxide and the final product; if the concentration is lower than 3M, the surface impurities may not be completely removed.
[0092] The alcohol solvent is mainly used to remove organic impurities (such as grease impurities) on the surface of the nickel foam sheet.
[0093] There is no particular limitation on the alcohol solvent, and it may be an alcohol solvent commonly used in the art, for example, alcohol, glycol, etc., such as ethanol or ethylene glycol, preferably ethanol.
[0094] The water is mainly used to remove residual liquid on the surface of the nickel foam sheet.
[0095] There is no particular limitation on the water, and it can be water commonly used in the art. For example, the water can be deionized water, ion exchange water, distilled water, ultrapure water, preferably ultrapure water.
[0096] The above three cleaning agents can be used for cleaning once or multiple times respectively.
[0097] If ultrasonic cleaning with the above three cleaning agents is not performed, the residual impurities on the surface of the nickel foam sheet may adversely affect the stability, morphology and overall performance of subsequent material synthesis.
[0098] Step (b) Growth of Cobalt-Copper Double Hydroxide
[0099] Step (b) comprises:
[0100] (b1) dissolving a stabilizer, a reaction aid, a soluble cobalt salt and a soluble copper salt in a first solvent to obtain a first solution, and placing the pretreated nickel foam sheet in the first solution, wherein the molar ratio of the soluble cobalt salt to the soluble copper salt is 1:5 to 1:7,
[0101] (b2) then performing a hydrothermal reaction to grow cobalt-copper double metal hydroxide on the inner and outer surfaces of the pores of the pretreated nickel foam sheet,
[0102] (b3) The obtained product is then washed to obtain an intermediate.
[0103] Step (b1)
[0104] First, a stabilizer, a reaction aid, a soluble cobalt salt and a soluble copper salt in a specific molar ratio are added to a first solvent, and stirred to dissolve to obtain a first solution, and the pretreated nickel foam sheet is placed in the first solution to obtain a mixture. The molar ratio of the soluble cobalt salt to the soluble copper salt is 1:5 to 1:7.
[0105] The first solution can be prepared by conventional techniques.
[0106] The first solvent is mainly used to dissolve stabilizers, reaction aids, soluble cobalt salts, and soluble copper salts.
[0107] There is no particular limitation on the first solvent, and it can be a commonly used solvent in the art. For example, the first solvent can be at least one of ultrapure water, deionized water, ethanol, and acetone, preferably a mixture of ultrapure water and ethanol.
[0108] The stabilizer is mainly used to prevent the agglomeration of cobalt-copper double metal hydroxide nanoparticles and maintain the dispersibility and stability of the nanomaterial.
[0109] There is no particular limitation on the stabilizer, and it can be a stabilizer commonly used in the art. For example, the stabilizer can be at least one of urea, urea, and ethylenediamine, preferably urea.
[0110] If no stabilizer is added, the synthesis of cobalt-copper double hydroxide will be uneven and agglomerated.
[0111] The reaction aid is mainly used to help control the crystal morphology and particle size of the cobalt-copper double metal hydroxide.
[0112] There is no particular limitation on the reaction aid, and it can be a commonly used reaction aid in the art. For example, the reaction aid can be at least one of ammonium fluoride and ammonium chloride, preferably ammonium fluoride.
[0113] If no reaction aid is added, the crystal morphology and particle size of the obtained cobalt-copper double hydroxide will be uncontrollable.
[0114] The soluble cobalt salt is primarily present as a source of cobalt.
[0115] There is no particular limitation on the soluble cobalt salt, and it can be a soluble cobalt salt commonly used in the art. For example, the soluble cobalt salt can be at least one of cobalt nitrate, cobalt sulfate, and cobalt chloride, preferably cobalt nitrate.
[0116] The soluble copper salt is present primarily as a copper source.
[0117] There is no particular limitation on the soluble copper salt, and it can be a soluble copper salt commonly used in the art. For example, the soluble copper salt can be at least one of copper nitrate, copper sulfate, and copper chloride, preferably copper nitrate.
[0118] Relative to 1g pretreated nickel foam sheet,
[0119] The amount of the stabilizer can be 0.01 to 0.1 g, preferably 0.05 to 0.08 g.
[0120] The dosage of the reaction aid can be 0.01 to 0.1 g, preferably 0.04 to 0.08 g.
[0121] The total amount of the soluble cobalt salt and the soluble copper salt may be 1 to 2 mmol, preferably 1.2 to 1.6 mmol.
[0122] The volume of the first solvent may be 20 to 50 ml, preferably 25 to 35 ml.
[0123] The molar ratio of the soluble cobalt salt to the soluble copper salt may be 1:5 to 1:7. By using the above specific molar ratio, a hydrogen evolution catalyst for water electrolysis with significantly improved durability and electrocatalytic activity at high current density may be prepared. Preferably, the molar ratio of the soluble cobalt salt to the soluble copper salt may be 1:5.5 to 1:6.5, more preferably, 1:6.
[0124] If the molar ratio of the soluble cobalt salt to the soluble copper salt is outside the above range, the performance of the resulting catalyst will be significantly reduced.
[0125] Step (b2)
[0126] Then, the mixture obtained in step (b1) is subjected to a hydrothermal reaction to grow cobalt-copper double metal hydroxide on the inner and outer surfaces of the pores of the pretreated nickel foam sheet.
[0127] The hydrothermal reaction is a common synthesis method in the art. For example, the hydrothermal reaction can be carried out in an autoclave. Specifically, the autoclave can be a 50 ml stainless steel autoclave lined with polytetrafluoroethylene. The heating method can be oven heating. The atmosphere of the hydrothermal reaction can be an air atmosphere.
[0128] The heating temperature of the hydrothermal reaction may be 80 to 160°C, preferably 100 to 140°C, and more preferably 110 to 130°C.
[0129] If the heating temperature is lower than 80°C, the reaction rate is slow or even no reaction occurs; if the heating temperature is higher than 160°C, the reaction rate is too fast, the surface morphology cannot be controlled, and the accumulated materials are likely to clog the internal pores of the nickel foam sheet.
[0130] When the heating temperature is within the above range, a suitable reaction rate can be obtained to form a suitable surface morphology.
[0131] The heating time of the hydrothermal reaction is 4 to 12 hours, preferably 6 to 10 hours, and more preferably 7 to 9 hours.
[0132] If the heating time is less than 4 h, less cobalt copper double hydroxide is synthesized and the performance is less affected, while if the heating time is more than 12 h, the process efficiency will be reduced and the production cost will be increased.
[0133] When the heating time is within the above range, sufficient cobalt-copper double hydroxide can be obtained at a lower cost.
[0134] Cobalt-copper double hydroxide is an excellent catalytically active component that can provide active sites for hydrogen evolution reaction.
[0135] Step (b3)
[0136] The obtained product is then washed to obtain an intermediate.
[0137] The cleaning can be performed by using two cleaning agents, an organic cleaning agent and water, respectively in this order.
[0138] The organic cleaning agent is mainly used to clean the residual organic solution on the surface of the intermediate.
[0139] There is no particular limitation on the organic cleaning agent, and it can be alcohol materials and ketone materials commonly used in the art. For example, the organic cleaning agent can be ethanol, ethylene glycol, acetone, methyl isobutyl ketone, preferably ethanol and acetone. If multiple organic cleaning agents are used, the various organic cleaning agents should be used separately and cannot be mixed, so as to clean the obtained products separately.
[0140] The water is mainly used to remove residual liquid on the surface of the obtained product and cobalt copper double metal hydroxide loosely connected on the surface.
[0141] There is no particular limitation on the water, and it can be water commonly used in the art. For example, the water can be at least one of deionized water, ion exchange water, distilled water, and ultrapure water, preferably ultrapure water.
[0142] The above two cleaning agents can be used for cleaning once or multiple times respectively.
[0143] If the above two cleaning agents are not used for cleaning, the residual impurities on the surface of the intermediate (such as the solids left after the residual liquid on the surface dries, and the hydroxides loosely connected on the surface) will have an adverse effect on the stability, morphology and overall performance of the subsequent material synthesis.
[0144] In the obtained intermediate, the grown cobalt-copper double hydroxide is located on the inner and outer surfaces of the pores of the nickel foam sheet (i.e., on all surfaces of the nickel foam sheet) and forms a thin layer covering the nickel foam sheet. In addition, the intermediate has a porous structure and has pores corresponding to the nickel foam sheet.
[0145] Optionally, the product may be dried after washing. The drying may be performed by vacuum drying. The drying temperature may be 40 to 60° C., for example, 45 to 50° C. The drying time may be 8 to 24 hours, for example, 10 to 12 hours.
[0146] Step (c) Growth of Graphdine
[0147] Step (c) comprises:
[0148] (c1) preparing a mixture comprising a second solvent and hexa(trimethylsilylethynyl)benzene as a graphyne precursor, and adding a diluent and a buffer to obtain a second solution, and adding Cu foil and the intermediate to the second solution,
[0149] (c2) then performing a heating reaction under an inert atmosphere to grow graphyne on the intermediate,
[0150] (c3) The obtained product is then washed and dried to obtain the hydrogen evolution catalyst for water electrolysis.
[0151] Step (c1)
[0152] A mixture including a second solvent and hexa(trimethylsilylethynyl)benzene as a graphyne precursor is prepared, and then a diluent and a buffer are added to obtain a second solution, and Cu foil and the intermediate are added to the second solution.
[0153] The second solution can be prepared by conventional technical means. The second solution is usually a colorless and transparent solution.
[0154] The second solvent is mainly used to dissolve hexa(trimethylsilylethynyl)benzene as a graphyne precursor.
[0155] The second solvent is not particularly limited and may be a commonly used solvent in the art, for example, at least one of pyridine, self-bipyridine, polyvinylpyridine, and polymer-bonded 4-(dimethylamino)-pyridine, preferably pyridine.
[0156] The diluent is used to dilute the second solution, thereby controlling the reaction rate.
[0157] The diluent is not particularly limited and may be a commonly used diluent in the art, for example, at least one of acetone, methanol, ethanol, ethylene glycol, isopropanol, N,N-dimethylformamide, carbon tetrachloride, dimethyl sulfoxide, and ultrapure water, preferably acetone.
[0158] If no diluent is used, the solution concentration is too high, the reaction rate is too fast, the morphology of the grown graphyne is difficult to control, and it is easy to clog the internal pores of the nickel foam sheet.
[0159] The buffer is used to stabilize the pH value of the solution during the reaction and prevent the polarity of the solution from increasing too quickly, so as to obtain a more stable and uniform graphyne product.
[0160] The buffer is not particularly limited and may be a commonly used buffer in the art, for example, at least one of tetramethylethylenediamine, bicarbonate buffer, and acetic acid / sodium acetate buffer, preferably tetramethylethylenediamine.
[0161] If a buffer is not used, the pH of the solution may be uncontrollable, the polarity of the solution may increase too quickly, and the synthesis of graphyne may be uneven and unstable.
[0162] The Cu foil is used as a catalyst to catalyze the reaction of synthesizing graphyne. The Cu foil and the intermediate are usually placed separately in the second solution.
[0163] Relative to 1g pretreated nickel foam sheet,
[0164] The amount of the second solvent can be 30 to 120 ml, preferably 40 to 70 ml.
[0165] The amount of hexa(trimethylsilylethynyl)benzene used can be 0.05 to 0.1 mmol, preferably 0.06 to 0.09 mmol, and is used by dissolving in the second solvent.
[0166] The volume ratio of the diluent to the buffer may be 50:1 to 200:1, preferably 80:1 to 130:1.
[0167] The amount of the diluent can be 50 to 120 ml, preferably 80 to 110 ml.
[0168] The amount of the Cu foil may be 0.5 to 2 g, preferably 0.8 to 1.5 g.
[0169] Step (c2)
[0170] A heating reaction is then performed under an inert atmosphere to grow graphyne on the intermediate.
[0171] During the synthesis of graphyne, an inert atmosphere is used to minimize the occurrence of side reactions.
[0172] There is no particular limitation on the inert atmosphere, and it can be an inert atmosphere commonly used in the art. For example, the inert atmosphere can be at least one of a nitrogen atmosphere and an argon atmosphere, preferably argon.
[0173] If the reaction is not carried out under an inert atmosphere, the conversion rate of graphyne will be extremely low, and there will be many side reactions, and the target material cannot be obtained.
[0174] During the synthesis of graphyne, heating can provide a more suitable reaction temperature for the synthesis of graphyne.
[0175] The heating method can be a heating method commonly used in the art. For example, the reaction container used can be a 200 ml three-necked flask, and the heating method can be heating with an asbestos heating jacket.
[0176] The heating temperature of the heating reaction may be 40 to 60°C, preferably 45 to 55°C.
[0177] If the heating temperature is lower than 40°C, the reaction rate is slow or even no reaction occurs; if the heating temperature is higher than 60°C, a large number of side reactions occur, the graphyne yield is low and a large number of by-products are produced.
[0178] When the heating temperature is within the above range, a suitable reaction rate can be obtained, the yield of graphyne can be guaranteed, and the occurrence of side reactions can be avoided.
[0179] The heating time of the heating reaction is 20 to 48 hours, preferably 22 to 30 hours, and more preferably 24 to 28 hours.
[0180] If the heating time is less than 20 hours, less graphyne will be synthesized and the active ingredients cannot be fully protected. If the heating time is more than 48 hours, too much graphyne will be synthesized, affecting the action of the active ingredients, and the accumulated graphyne material will easily clog the internal pores of the catalyst.
[0181] When the heating time is within the above range, a suitable amount of graphyne synthesis can be obtained.
[0182] As mentioned above, Graphdiyne, as a protective agent, can effectively enhance the chemical and mechanical stability of cobalt-copper double hydroxides while maintaining their excellent electrocatalytic activity. In addition, Graphdiyne also promotes rapid charge transfer through its unique electronic structure.
[0183] Step (c3)
[0184] Then, the obtained product is washed and dried to obtain the hydrogen evolution catalyst for water electrolysis.
[0185] The cleaning method can be carried out in the same manner as step (b3).
[0186] The material can be dried by conventional processes, and the drying method can be vacuum drying to prevent the cobalt copper double metal hydroxide from reacting with oxygen in the air.
[0187] The drying temperature may be 40 to 60°C, for example, 45 to 50°C.
[0188] The drying time may be 8 to 24 hours, for example, 10 to 12 hours.
[0189] The obtained hydrogen evolution catalyst has a porous structure and has pores corresponding to the nickel foam sheet. In the inner surface part and the outer surface part of the pore of the hydrogen evolution catalyst, graphyne is located on the cobalt copper double metal hydroxide and forms a thin layer covering the cobalt copper double metal hydroxide. Specifically, the inner surface part and the outer surface part of the pore of the hydrogen evolution catalyst have a stacked structure formed by the nickel foam sheet, the cobalt copper double metal hydroxide and graphyne.
[0190] 2. Hydrogen evolution catalyst for water electrolysis
[0191] According to a second aspect of the present invention, a hydrogen evolution catalyst for water electrolysis is provided, which can be prepared by the above method, and the hydrogen evolution catalyst comprises a nickel foam sheet, a cobalt-copper double metal hydroxide and graphyne.
[0192] The pores in the hydrogen evolution catalyst correspond to the pores in the nickel foam sheet. In addition, in the hydrogen evolution catalyst, cobalt-copper double metal hydroxide is located on the inner and outer surfaces of the pores of the nickel foam sheet to coat the nickel foam sheet, and graphyne is located on the cobalt-copper double metal hydroxide to coat the cobalt-copper double metal hydroxide.
[0193] The thickness of the cobalt-copper double hydroxide and the graphyne may be respectively nanometer-scale.
[0194] The detailed description of nickel foam sheet, cobalt-copper double hydroxide and graphyne can be found above.
[0195] Cobalt-copper double hydroxide is usually used as an oxygen evolution catalyst. However, through in-depth research, the inventors of the present application found that by controlling the molar ratio of cobalt to copper, cobalt-copper double hydroxide can also be used as a hydrogen evolution catalyst.
[0196] In addition, in the prior art, glassy carbon electrodes are usually used as electrodes for loading catalytic active components. However, if cobalt-copper double hydroxide is loaded on the glassy carbon electrode, during the hydrogen evolution reaction, the cobalt-copper double hydroxide is easily peeled off due to the continuous evolution of hydrogen.
[0197] Nickel foam is a porous, high-surface-area material with excellent electrical conductivity and corrosion resistance, and can also be used to load catalytically active components. A catalyst having a binary composite structure is obtained by loading a cobalt-copper double hydroxide having a specific cobalt-copper molar ratio on a nickel foam. The internal pores of the nickel foam can significantly increase the specific surface area of the cobalt-copper double hydroxide, thereby providing more active sites. However, a long period of hydrogen evolution reaction still causes the cobalt-copper double hydroxide in the surface of the catalyst to peel off, thereby reducing the catalytic performance.
[0198] Based on the above binary composite structure, the present invention further grows graphyne on the surface of the cobalt-copper double hydroxide to prevent the cobalt-copper double hydroxide from peeling off, thereby obtaining a novel hydrogen evolution catalyst for water electrolysis.
[0199] The hydrogen evolution catalyst of the present invention is a porous sheet material and has a unique ternary composite structure. Through the synergistic effect of the nickel foam sheet, the cobalt-copper double metal hydroxide with a specific cobalt-copper molar ratio and graphyne, it not only improves the conductivity of the catalytically active component (cobalt-copper double metal hydroxide), but also provides it with a larger reaction surface area, thereby significantly improving the electrocatalytic activity.
[0200] Example
[0201] Hereinafter, the present invention will be described in detail with reference to embodiments to specifically describe the present invention. However, embodiments of the present invention may be modified into various other forms, and the scope of the present invention should not be construed as being limited to the embodiments described below. Embodiments of the present invention are provided to more fully describe the present invention to those of ordinary skill in the art.
[0202] The experimental methods in the following examples, unless otherwise specified, are generally conventional conditions in the art or conditions recommended by the manufacturer; the raw materials and equipment used are all commercially available from conventional markets, etc., unless otherwise specified.
[0203] Example 1
[0204] The hydrogen evolution catalyst for water electrolysis is prepared by the following steps.
[0205] Step (a) Pretreatment
[0206] The commercially available original nickel foam material was cut into nickel foam sheets of 1.5 cm in length × 1 cm in width × 0.03 cm in thickness, and then ultrasonically treated in 3.0 M HCl solution, ethanol, and ultrapure water for 15 minutes each to remove surface impurities. The pretreated nickel foam sheet weighed 1 g.
[0207] Step (b) Growth of Cobalt-Copper Double Hydroxide
[0208] 0.060 g of urea as a stabilizer, 0.076 g of NH4F as a reaction aid, 0.052 g (0.18 mmol) of Co(NO3)2·6H2O and 0.27 g (1.08 mmol) of Cu(NO3)2·3H2O (the molar ratio of cobalt salt to copper salt is 1:6, and the total amount is 1.25 mmol) are dissolved in a mixed solution of 25 ml of ultrapure water and 5 ml of ethanol to obtain a first solution, and the pretreated nickel foam sheet is placed in the first solution to obtain a mixture.
[0209] The mixture is then placed in a high-pressure reactor with a polytetrafluoroethylene liner and subjected to a hydrothermal reaction at 120° C. for 8 hours, thereby growing cobalt-copper double metal hydroxides on the inner and outer surfaces of the pores of the pretreated nickel foam sheet.
[0210] The obtained product was then washed three times with acetone and ultrapure water respectively to obtain an intermediate.
[0211] Step (c) Growth of Graphdine
[0212] 0.046 g (0.07 mmol) of (hexa(trimethylsilylethynyl)benzene) as a graphyne precursor was dissolved in 50 ml of pyridine as a second solvent, and then 100 ml of acetone as a diluent and 1 ml of tetramethylethylenediamine as a buffer were added to obtain a second solution, and 1 g of Cu foil and the intermediate were added to the second solution.
[0213] Then, the mixture was heated to 50° C. under an argon atmosphere and reacted for 25 hours to grow graphyne on the intermediate.
[0214] The obtained material was then washed three times with acetone and ultrapure water respectively, and dried in vacuum at 40° C. for 10 h to obtain a hydrogen evolution catalyst for water electrolysis.
[0215] Example 2
[0216] A hydrogen evolution catalyst for water electrolysis was prepared in the same manner as in Example 1, except that the molar ratio of the cobalt salt to the copper salt in step (b) was changed to 1:5, and the total amount of the cobalt salt and the copper salt was kept unchanged.
[0217] Example 3
[0218] A hydrogen evolution catalyst for water electrolysis was prepared in the same manner as in Example 1, except that the molar ratio of the cobalt salt to the copper salt in step (b) was changed to 1:7, and the total amount of the cobalt salt and the copper salt was kept unchanged.
[0219] Comparative Example 1
[0220] A hydrogen evolution catalyst for water electrolysis was prepared in the same manner as in Example 1, except that step (c) was omitted.
[0221] Comparative Example 2
[0222] A hydrogen evolution catalyst for water electrolysis was prepared in the same manner as in Example 1, except that the molar ratio of the cobalt salt to the copper salt in step (b) was changed to 1:4, and the total amount of the cobalt salt and the copper salt was kept unchanged.
[0223] Comparative Example 3
[0224] A hydrogen evolution catalyst for water electrolysis was prepared in the same manner as in Example 1, except that the molar ratio of the cobalt salt to the copper salt in step (b) was changed to 1:8, and the total amount of the cobalt salt and the copper salt was kept unchanged.
[0225] Comparative Example 4
[0226] A hydrogen evolution catalyst for electrolysis of water is prepared in the same manner as in Example 1, except that the hydroxide grown in step (b) is changed to (a) iron-cobalt bimetallic hydroxide, (b) iron-nickel bimetallic hydroxide, (c) iron-copper bimetallic hydroxide, (d) cobalt-nickel bimetallic hydroxide, and (e) nickel-copper bimetallic hydroxide, respectively, and the molar ratio of the bimetal in step (b) is changed to 10:1, 5:1, 1:1, 1:5, and 1:10, respectively, and the total amount of cobalt salt and copper salt is kept unchanged.
[0227] Specifically, the above series of comparative examples are referred to as Comparative Examples 4(a) to 4(e), respectively.
[0228] Experimental Example 1 Overpotential (electrocatalytic activity) measurement at high current density
[0229] An electrochemical workstation (manufactured by Shanghai Chenhua, model CHI 660E) was used to perform electrochemical tests on the hydrogen evolution catalysts for electrolysis of water of Examples 1 to 3 and Comparative Examples 1 to 4. Specifically, each hydrogen evolution catalyst for electrolysis of water was clamped on an electrode clamp, and a three-electrode system (hydrogen evolution catalyst for electrolysis of water as a working electrode, a carbon rod as a counter electrode, a calomel electrode as a reference electrode, and a 1.0 M KOH solution as an electrolyte solution) was used to measure and obtain a linear sweep voltammetric curve.
[0230] First, according to the above linear sweep voltammetry curves, the overpotentials of the hydrogen evolution catalysts for water electrolysis of Examples 1 to 3 and Comparative Examples 1 to 3 are obtained, as shown in Table 1 below.
[0231] Table 1
[0232]
[0233] It can be seen from Table 1 that at two high current densities (specifically 50 mA cm -2 and 100mA·cm -2 ), the overpotentials of Examples 1 to 3 are significantly lower than those of Comparative Examples 1 to 3, indicating that the electrocatalytic activity of the hydrogen evolution catalysts for water electrolysis of Examples 1 to 3 is excellent.
[0234] In addition, it can be seen that for the hydrogen evolution catalyst for water electrolysis containing graphyne in Example 1, its -2 and 100mA·cm -2 The overpotential under the current density is significantly lower than that of the hydrogen evolution catalyst for water electrolysis without graphyne in Comparative Example 1.
[0235] It is thus confirmed that in the hydrogen evolution catalyst for water electrolysis as a ternary composite material of the present invention, the coating of graphyne can significantly reduce the overpotential of the hydrogen evolution catalyst for water electrolysis at high current density to obtain more excellent electrocatalytic activity.
[0236] In addition, it can be seen that for the hydrogen evolution catalysts for water electrolysis prepared by controlling the molar ratio of cobalt salt to copper salt in the specific range of 1:5 to 1:7 in Examples 1 to 3, they have a high conductivity at 50 mA·cm -2 and 100mA·cm -2 The overpotential at a high current density is significantly lower than that of the hydrogen evolution catalyst for water electrolysis in Comparative Examples 2 and 3 (the molar ratios of the cobalt salt and the copper salt are 1:4 and 1:8, respectively).
[0237] It is thus confirmed that the hydrogen evolution catalyst for water electrolysis prepared within a specific molar ratio range of cobalt salt to copper salt according to the present invention can have excellent electrocatalytic activity at high current density.
[0238] Secondly, similarly, based on the above linear sweep voltammetry curves, the overpotentials of the hydrogen evolution catalysts for water electrolysis of Comparative Examples 4(a) to 4(e) at different bimetallic molar ratios were obtained, as shown in Tables 2(a) to 2(e) below.
[0239] Table 2(a)
[0240]
[0241] Table 2(b)
[0242]
[0243] Table 2(c)
[0244]
[0245] Table 2(d)
[0246]
[0247] Table 2(e)
[0248]
[0249] As can be seen from Tables 2(a) to 2(e), for the catalysts for hydrogen evolution by electrolysis of water of Comparative Example 4 (in which bimetallic hydroxides of different types and with different ratios are grown on nickel foam sheets), their performance at 50 mA cm -2 and 100mA·cm -2 The overpotential at high current density is obviously too high and has no application value.
[0250] It is thus confirmed that the catalyst for hydrogen evolution by water electrolysis of the present invention can have excellent electrocatalytic activity at high current density by growing a cobalt-copper double hydroxide having a specific cobalt-copper molar ratio on a nickel foam sheet.
[0251] Experimental Example 2 Durability Measurement at High Current Density
[0252] The same instrument as that of Experimental Example 1 was used to test the hydrogen evolution catalysts for water electrolysis of Example 1 and Comparative Example 1 for 24 hours at a constant current of 0.1 A. The linear sweep voltammetric curves were measured before and after the test, and the obtained overpotentials are shown in Tables 3 and 4 below.
[0253] Table 3 Current density 50mA·cm -2 Overpotential comparison under
[0254]
[0255] Table 4 Current density is 100 mA cm -2 Overpotential comparison under
[0256]
[0257] It can be seen from Tables 3 and 4 that compared with Comparative Example 1, after 24 hours of testing at a constant current of 0.1 A, when the current density is 50 mA·cm -2 and 100mA·cm -2 When the overpotential of the hydrogen evolution catalyst for water electrolysis of Example 1 is increased, the overpotential increase is significantly smaller.
[0258] This confirmed that the hydrogen evolution catalyst for water electrolysis of the present invention can have excellent durability at a high current density by coating graphyne on the cobalt-copper double hydroxide.
[0259] Experimental Example 3 Scanning Electron Microscope Observation
[0260] The surface morphology of the hydrogen evolution catalysts for water electrolysis obtained in Comparative Example 1 and Example 1 was observed using a scanning electron microscope. The results are shown in Figure 1 and 2 middle.
[0261] from Figure 1 It can be seen that in Comparative Example 1, a layer of granular cobalt-copper double hydroxide is uniformly grown on the surface of the nickel foam sheet. However, due to the uneven force on the cobalt-copper double hydroxide during the particle aggregation process, some small gaps inevitably appear, which can easily cause the cobalt-copper double hydroxide to fall off during the long-term high-current hydrogen evolution process.
[0262] In contrast, from Figure 2 It can be seen that Example 1 further synthesizes a layer of granular graphyne on the surface of the cobalt-copper double hydroxide of Comparative Example 1, thereby forming a protective layer on the surface of the cobalt-copper double hydroxide, which effectively prevents the cobalt-copper double hydroxide from falling off. It is thus confirmed that the present invention successfully synthesizes graphyne uniformly on the cobalt-copper double hydroxide, and the resulting hydrogen evolution catalyst for water electrolysis can have excellent durability at high current density.
[0263] Although the preferred embodiments of the present invention have been disclosed for illustrative purposes, those skilled in the art will appreciate that various modifications, additions and substitutions are possible, without departing from the scope and spirit of the invention as disclosed in the accompanying claims.
Claims
1. A method for preparing a hydrogen evolution catalyst for water electrolysis, the method comprising the steps of: (a) preparing a nickel foam sheet, and cleaning the nickel foam sheet to remove surface impurities; (b) dissolving a stabilizer, a reaction aid, a soluble cobalt salt and a soluble copper salt in a first solvent to obtain a first solution, and placing the pretreated nickel foam sheet in the first solution, wherein the molar ratio of the soluble cobalt salt to the soluble copper salt is 1:5 to 1:7, Then, a hydrothermal reaction is performed to grow cobalt-copper double metal hydroxide on the inner and outer surfaces of the pores of the pretreated nickel foam sheet. Then, the obtained product is washed to obtain an intermediate; (c) preparing a mixture comprising a second solvent and hexa(trimethylsilylethynyl)benzene as a graphyne precursor, and adding a diluent and a buffer to obtain a second solution, and adding Cu foil and the intermediate to the second solution, Then, a heating reaction is carried out under an inert atmosphere to grow graphene on the intermediate. Then, the obtained product is washed and dried to obtain the hydrogen evolution catalyst for water electrolysis.
2. The method according to claim 1, wherein: In step (a), The prepared nickel foam sheet has a length of 1 to 1.5 cm, a width of 1 to 1.5 cm, a thickness of 0.03 to 0.05 cm, and In the cleaning, the nickel foam sheet is ultrasonically treated with HCl solution, alcohol solvent and water in sequence. The alcohol solvent is at least one of ethanol and ethylene glycol, The water is at least one of deionized water, ion exchange water, distilled water and ultrapure water.
3. The method according to claim 1, wherein: In step (b), In the first solution, the stabilizer is at least one of urea, urea, and ethylenediamine. The reaction aid is at least one of ammonium fluoride and ammonium chloride, The soluble cobalt salt is at least one of cobalt nitrate, cobalt sulfate and cobalt chloride. The soluble copper salt is at least one of copper nitrate, copper sulfate and copper chloride. The first solvent is at least one of ultrapure water, deionized water, ethanol and acetone.
4. The method according to claim 1, wherein: In step (b), Relative to 1g pretreated nickel foam sheet, The amount of the stabilizer is 0.01 to 0.1 g. The dosage of the reaction aid is 0.01 to 0.1 g. The total amount of the soluble cobalt salt and the soluble copper salt is 1 to 2 mmol, The volume of the first solvent is 20-50 ml.
5. The method according to claim 1, wherein: In step (b), The temperature of the hydrothermal reaction is 80-160°C. The hydrothermal reaction time is 4 to 12 hours. The cleaning is performed by using an organic cleaning agent and water in sequence.
6. The method according to claim 1, wherein: In step (c), The second solvent is pyridine or a pyridine derivative, wherein the pyridine derivative is at least one selected from bipyridine, polyvinyl pyridine, and polymer-bonded 4-(dimethylamino)-pyridine. The diluent is at least one of acetone, methanol, ethanol, ethylene glycol, isopropanol, N,N-dimethylformamide, carbon tetrachloride, dimethyl sulfoxide, and ultrapure water. The buffer is at least one of tetramethylethylenediamine, bicarbonate buffer, and acetic acid / sodium acetate buffer.
7. The method according to claim 1, wherein: In step (c), Relative to 1g pretreated nickel foam sheet, The dosage of the second solvent is 50-100 ml. The amount of hexa(trimethylsilylethynyl)benzene used is 0.05-0.1 mmol, and it is used by dissolving in the second solvent. The volume ratio of the diluent to the buffer is 50:1 to 200:1, The usage amount of the diluent is 50 to 120 ml. The amount of the Cu foil is 0.5-2 g.
8. The method according to claim 1, wherein: In step (c), The inert atmosphere is at least one of an argon atmosphere and a nitrogen atmosphere. The temperature of the heating reaction is 40-60°C, The heating reaction time is 20 to 48 hours. The cleaning is performed by using an organic cleaning agent and water in sequence. The drying is vacuum drying, the drying temperature is 40 to 60° C., and the drying time is 8 to 24 hours.
9. A hydrogen evolution catalyst for water electrolysis, which is prepared by the method according to claim 1, wherein the hydrogen evolution catalyst comprises a nickel foam sheet, a cobalt-copper double metal hydroxide and graphyne, in, The cobalt-copper double metal hydroxide is located on the inner and outer surfaces of the pores of the nickel foam sheet. The graphyne is located on the cobalt-copper double hydroxide, and The pores in the hydrogen evolution catalyst correspond to the pores in the nickel foam sheet. 10 . The hydrogen evolution catalyst for water electrolysis according to claim 9 , wherein the hydrogen evolution catalyst is used as a catalyst for the hydrogen evolution reaction and also as a cathode of an electrolytic cell.