Preparation method of efficient chlorine evolution electrode

By adding aluminate and silicate to the coating solution formulation, a porous electrode surface is constructed, which solves the problems of low electrode selectivity and difficulty in desorbing chlorine bubbles, and achieves a high-efficiency improvement in the electrolytic preparation of hypochlorous acid.

CN118957669APending Publication Date: 2024-11-15HUNAN XINNANFANG CULTURE SERVICE CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411186336.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-05-28
Filing Date
2024-08-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In existing electrolytic methods for preparing hypochlorous acid, the electrodes exhibit low selectivity, decreased activity, and poor stability in a limited chloride environment. Furthermore, the generated chlorine bubbles are difficult to desorb in a timely manner, affecting the electrolysis efficiency.

Method used

Aluminate and silicate are added to the coating formulation, and a porous electrode surface is constructed by treatment with sodium hydroxide and hydrofluoric acid to achieve rapid detachment of chlorine bubbles.

Benefits of technology

The electrolysis efficiency was improved by more than 20%, and the purity and stability of hypochlorous acid solution prepared by electrolysis were enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957669A_ABST
    Figure CN118957669A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an efficient chlorine evolution electrode, which specifically comprises the following steps: step 1, carrying out sand blasting on the surface of a titanium substrate to obtain a matrix, and cleaning and drying the matrix; step 2, adding noble metal salt, a dispersing agent, a stabilizing agent and a pore-forming agent precursor into a reactor, and reacting to obtain a coating solution; 3, coating liquid coating and high-temperature sintering are repeatedly carried out for multiple times till the coating thickness meeting the requirement is obtained; step 4, adding the matrix sintered and cured in the step 3 into a NaOH solution for boiling, and then performing ultrasonic cleaning with water until the surface is free of alkalinity; step 5, immersing the matrix treated in the step 4 into hydrofluoric acid for ultrasonic reaction, and then performing ultrasonic cleaning with water until the surface is free of acidity; and 6, the matrix treated in the step 5 is subjected to high-temperature sintering again. The porous electrode surface can be constructed, so that chlorine bubbles generated in the electrolysis process can be quickly separated from the electrode surface, and the electrolysis efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrode preparation, and in particular relates to a method for preparing a high-efficiency chlorine evolution electrode. Background Art

[0002] Hypochlorous acid is an oxygen-containing acid of the element chlorine with the chemical formula HClO. Hypochlorous acid is mainly used as a disinfectant and is widely used to disinfect surfaces, contaminated items such as fabrics, water, fruits and vegetables, and tableware, as well as indoor air, surfaces of secondary water supply equipment and facilities, hands, skin, and mucous membranes. Common methods for preparing hypochlorous acid include: (1) electrolysis, i.e., preparing hypochlorous acid by electrolyzing low-concentration hydrochloric acid or sodium chloride solutions; (2) chemical reaction, i.e., producing hypochlorous acid by chemical reagent reaction.

[0003] Since the production of hypochlorous acid by electrolysis has the advantages of safety, low cost and high purity, research on the preparation of hypochlorous acid disinfectant by electrolysis has been devoted to the production of hypochlorous acid solution without byproducts. However, the practical electrolytic electrodes currently have problems of low selectivity, decreased activity and poor stability in limited chloride environments. In the past few years, many design strategies have been reported to improve the performance of electrocatalysts in electrolysis, but the generated chlorine bubbles cannot be desorbed from the electrode surface in time, which seriously affects the electrolysis efficiency. Therefore, it is necessary to take measures to accelerate the desorption of bubbles from the electrolytic anode surface. Summary of the invention

[0004] In view of the above problems, the present invention provides a method for preparing a high-efficiency chlorine evolution electrode. The present invention adds aluminate and silicate to the coating liquid formula, and then uses sodium hydroxide and hydrofluoric acid to remove aluminum and silicon elements to construct a porous electrode surface, so that chlorine bubbles generated during the electrolysis process can quickly detach from the electrode surface, thereby improving the electrolysis efficiency.

[0005] The present invention is achieved through the following technical solutions.

[0006] A method for preparing a high-efficiency chlorine evolution electrode, characterized in that the specific steps are as follows:

[0007] Step 1, sandblasting the surface of the titanium substrate to obtain a substrate, and cleaning and drying the substrate;

[0008] Step 2, adding the noble metal salt, dispersant, stabilizer and pore-forming agent precursor into the reactor, adjusting the pH value to 5-8, the temperature to 50-65° C., and reacting for 4-6 hours to obtain a coating solution;

[0009] Step 3, applying the coating liquid of step 2 to the surface of the substrate dried in step 1, and after the surface is dried, performing high-temperature sintering, and then repeating the coating liquid application and high-temperature sintering for multiple times until a coating thickness that meets the requirements is obtained;

[0010] Step 4, adding the substrate sintered and solidified in step 3 into a NaOH solution and boiling it, and then washing it with water ultrasound until the surface is free of alkalinity;

[0011] Step 5, immersing the substrate treated in step 4 in hydrofluoric acid for ultrasonic reaction, and then ultrasonically cleaning with water until the surface is free of acidity;

[0012] Step 6: sinter the substrate processed in step 5 again at high temperature.

[0013] Preferably, in step 1, the substrate is cleaned by pickling with 10% oxalic acid solution at a temperature of 90-100°C for 60-90 minutes, and the substrate is further cleaned by ultrasound after pickling for 20-40 minutes.

[0014] Preferably, in step 1, the drying is carried out by air drying or drying in a drying oven; the conditions for the drying in the drying oven are a drying temperature of 100 to 120° C. and a drying time of 20 to 30 minutes.

[0015] Preferably, in step 2, the noble metal salt is a mixture of ruthenium trichloride, tantalum pentachloride, chloroiridic acid and chloroplatinic acid.

[0016] Preferably, in step 2, the dispersant is one of ethanol, isopropanol or n-butanol.

[0017] Preferably, in step 2, the stabilizer is one of ethylene glycol, citric acid, PVP polymer, titanium tetrachloride, titanium trichloride and tetrabutyl titanate, or two of ethylene glycol, citric acid and PVP polymer.

[0018] Preferably, in step 2, the pore-forming agent precursor is a mixture of sodium aluminate and tetrabutyl silicate in a mass ratio of 1:1 to 5.

[0019] Preferably, in step 2, the ratio of the noble metal salt, the dispersant, the stabilizer and the pore-forming agent precursor by mass is 1:1-5:10-15:0.001-0.05.

[0020] Preferably, in step 2, the noble metal salt is a mixture of ruthenium trichloride, tantalum pentachloride, chloroiridic acid and chloroplatinic acid in a mass ratio of 1:0.1 to 1:0.1 to 1:0.1 to 0.5.

[0021] Preferably, in step 3, the high temperature sintering temperature is 250-450° C., and the sintering time is 10 min-15 min.

[0022] Preferably, in step 4, the concentration of NaOH is 40-60%wt, and the boiling time is 30-60min.

[0023] Preferably, in step 5, the concentration of hydrofluoric acid is 10 to 30% wt, and the ultrasonic reaction time is 30 to 60 min.

[0024] Preferably, in step 6, the high temperature sintering temperature is 450-550° C., and the sintering time is 10-15 minutes.

[0025] Compared with the prior art, the present invention has at least the following beneficial effects: by adding aluminate and silicate to the coating liquid formula, and then removing aluminum and silicon elements with sodium hydroxide and hydrofluoric acid, the present invention can successfully construct a microporous structure on the electrode surface, which not only does not affect the performance of the electrolytic electrode, but can also reduce the adsorption of chlorine bubbles on the electrode surface during the electrolysis process, so as to achieve the rapid detachment of chlorine bubbles generated during the electrolysis process from the electrode surface, thereby improving the electrolysis efficiency; according to testing, when preparing hypochlorous acid disinfectant by electrolysis, the present invention can improve the electrolysis efficiency by more than 20% compared with the conventional method. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The surface morphology of the pole piece is obtained using an optical microscope under the same magnification objective. DETAILED DESCRIPTION

[0027] The technical solutions in the present invention are described clearly and completely below. Obviously, the described embodiments are only a few embodiments of the present invention, not all embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] A method for preparing an efficient chlorine evolution electrode, the specific steps of which are as follows:

[0030] Step 1, sandblasting the surface of the titanium substrate to obtain a substrate, pickling with an oxalic acid solution having a concentration of 10%, the pickling temperature is 90° C., the time is 60 min, and after pickling, the substrate is further cleaned with ultrasound for 20 min, and then air-dried or dried in a drying oven; the drying oven is dried at a temperature of 120° C. and the drying time is 20 min;

[0031] Step 2, adding a noble metal salt, a dispersant, a stabilizer and a pore-forming agent precursor to a reactor, adjusting the pH value to 6 and the temperature to 50°C, and reacting for 4 hours to obtain a coating solution; wherein the noble metal salt is a mixture of ruthenium trichloride, tantalum pentachloride, chloroiridic acid and chloroplatinic acid in a mass ratio of 1:0.1:0.2:0.5; the dispersant is ethanol; the stabilizer is titanium tetrachloride; the pore-forming agent precursor is a mixture of sodium aluminate and tetrabutyl silicate in a mass ratio of 1:2; the mass ratio of the noble metal salt, the dispersant, the stabilizer and the pore-forming agent precursor is 1:5:10:0.05;

[0032] Step 3, applying the coating liquid of step 2 to the surface of the substrate dried in step 1, and after the surface is dried, high-temperature sintering is performed, and then the coating liquid coating and high-temperature sintering are repeated for multiple times until a coating thickness that meets the requirements is obtained; wherein the high-temperature sintering temperature is 250° C. and the sintering time is 15 minutes;

[0033] Step 4, adding the substrate sintered and solidified in step 3 into a 40%wt NaOH solution and boiling it for 30 minutes, and then washing it with water ultrasound until the surface is free of alkalinity;

[0034] Step 5, immersing the substrate treated in step 4 in hydrofluoric acid for ultrasonic reaction, and then ultrasonically cleaning with water until the surface is free of acidity; wherein the hydrofluoric acid concentration is 10%wt, and the ultrasonic reaction time is 30min;

[0035] Step 6: sinter the substrate processed in step 5 again at a temperature of 500° C. for 15 minutes.

[0036] Example 2

[0037] A method for preparing an efficient chlorine evolution electrode, the specific steps of which are as follows:

[0038] Step 1, sandblasting the surface of the titanium substrate to obtain a substrate, pickling with an oxalic acid solution having a concentration of 10%, the pickling temperature is 90° C., the time is 60 min, and after pickling, the substrate is further cleaned with ultrasound for 20 min, and then air-dried or dried in a drying oven; the drying oven is dried at a temperature of 120° C. and the drying time is 20 min;

[0039] Step 2, adding a noble metal salt, a dispersant, a stabilizer and a pore-forming agent precursor to a reactor, adjusting the pH value to 6 and the temperature to 50°C, and reacting for 4 hours to obtain a coating solution; wherein the noble metal salt is a mixture of ruthenium trichloride, tantalum pentachloride, chloroiridic acid and chloroplatinic acid in a mass ratio of 1:0.1:0.1:0.3; the dispersant is ethanol; the stabilizer is titanium tetrachloride; the pore-forming agent precursor is a mixture of sodium aluminate and tetrabutyl silicate in a mass ratio of 1:2; the ratio of the noble metal salt, the dispersant, the stabilizer and the pore-forming agent precursor in a mass ratio of 1:3:12:0.02;

[0040] Step 3, applying the coating liquid of step 2 to the surface of the substrate dried in step 1, and after the surface is dried, high-temperature sintering is performed, and then the coating liquid coating and high-temperature sintering are repeated for multiple times until a coating thickness that meets the requirements is obtained; wherein the high-temperature sintering temperature is 350° C. and the sintering time is 15 minutes;

[0041] Step 4, adding the substrate sintered and solidified in step 3 into a 40%wt NaOH solution and boiling it for 30 minutes, and then washing it with water ultrasound until the surface is free of alkalinity;

[0042] Step 5, immersing the substrate treated in step 4 in hydrofluoric acid for ultrasonic reaction, and then ultrasonically cleaning with water until the surface is free of acidity; wherein the hydrofluoric acid concentration is 10%wt, and the ultrasonic reaction time is 30min;

[0043] Step 6: The substrate processed in step 5 is sintered again at a temperature of 470° C. for 15 minutes.

[0044] Example 3

[0045] A method for preparing an efficient chlorine evolution electrode, the specific steps of which are as follows:

[0046] Step 1, sandblasting the surface of the titanium substrate to obtain a substrate, pickling with an oxalic acid solution having a concentration of 10%, the pickling temperature is 90° C., the time is 60 min, and after pickling, the substrate is further cleaned with ultrasound for 20 min, and then air-dried or dried in a drying oven; the drying oven is dried at a temperature of 120° C. and the drying time is 20 min;

[0047] Step 2, adding a noble metal salt, a dispersant, a stabilizer and a pore-forming agent precursor to a reactor, adjusting the pH value to 6 and the temperature to 50°C, and reacting for 4 hours to obtain a coating solution; wherein the noble metal salt is a mixture of ruthenium trichloride, tantalum pentachloride, chloroiridic acid and chloroplatinic acid in a mass ratio of 1:0.2:0.2:0.5; the dispersant is ethanol; the stabilizer is titanium tetrachloride; the pore-forming agent precursor is a mixture of sodium aluminate and tetrabutyl silicate in a mass ratio of 1:3.5; the mass ratio of the noble metal salt, the dispersant, the stabilizer and the pore-forming agent precursor is 1:3:7:0.005;

[0048] Step 3, applying the coating liquid of step 2 to the surface of the substrate dried in step 1, and after the surface is dried, high-temperature sintering is performed, and then the coating liquid coating and high-temperature sintering are repeated for multiple times until a coating thickness that meets the requirements is obtained; wherein the high-temperature sintering temperature is 250° C. and the sintering time is 15 minutes;

[0049] Step 4, adding the substrate sintered and solidified in step 3 into a 40%wt NaOH solution and boiling it for 30 minutes, and then washing it with water ultrasound until the surface is free of alkalinity;

[0050] Step 5, immersing the substrate treated in step 4 in hydrofluoric acid for ultrasonic reaction, and then ultrasonically cleaning with water until the surface is free of acidity; wherein the hydrofluoric acid concentration is 10%wt, and the ultrasonic reaction time is 30min;

[0051] Step 6: sinter the substrate processed in step 5 again at a temperature of 500° C. for 15 minutes.

[0052] Example 4

[0053] A method for preparing an efficient chlorine evolution electrode, the specific steps of which are as follows:

[0054] Step 1, sandblasting the surface of the titanium substrate to obtain a substrate, pickling with an oxalic acid solution having a concentration of 10%, the pickling temperature is 90° C., the time is 60 min, and after pickling, the substrate is further cleaned with ultrasound for 20 min, and then air-dried or dried in a drying oven; the drying oven is dried at a temperature of 120° C. and the drying time is 20 min;

[0055] Step 2, adding a noble metal salt, a dispersant, a stabilizer and a pore-forming agent precursor to a reactor, adjusting the pH value to 6 and the temperature to 50°C, and reacting for 4 hours to obtain a coating solution; wherein the noble metal salt is a mixture of ruthenium trichloride, tantalum pentachloride, chloroiridic acid and chloroplatinic acid in a mass ratio of 1:0.3:0.2:0.3; the dispersant is ethanol; the stabilizer is titanium tetrachloride; the pore-forming agent precursor is a mixture of sodium aluminate and tetrabutyl silicate in a mass ratio of 1:3.5; the mass ratio of the noble metal salt, the dispersant, the stabilizer and the pore-forming agent precursor is 1:2:12:0.05;

[0056] Step 3, applying the coating liquid of step 2 to the surface of the substrate dried in step 1, and after the surface is dried, high-temperature sintering is performed, and then the coating liquid coating and high-temperature sintering are repeated for multiple times until a coating thickness that meets the requirements is obtained; wherein the high-temperature sintering temperature is 300° C. and the sintering time is 15 minutes;

[0057] Step 4, adding the substrate sintered and solidified in step 3 into a 40%wt NaOH solution and boiling it for 30 minutes, and then washing it with water ultrasound until the surface is free of alkalinity;

[0058] Step 5, immersing the substrate treated in step 4 in hydrofluoric acid for ultrasonic reaction, and then ultrasonically cleaning with water until the surface is free of acidity; wherein the hydrofluoric acid concentration is 10%wt, and the ultrasonic reaction time is 30min;

[0059] Step 6: The substrate processed in step 5 is sintered again at a temperature of 550° C. for 15 minutes.

[0060] Example 5

[0061] Using commercially available ruthenium iridium titanium DSA electrodes as controls, the electrode sheets obtained in Examples 1-4 were used as anodes, and titanium sheets were used as cathodes to assemble a 10 positive 10 negative electrolytic cell. 10% sodium hydrochloride and 10% sodium chloride were electrolyzed (electrolyte flow rate 5 ml / min, current 3A), and water was used as a diluent after electrolysis (electrolyte volume: diluent volume = 1:500). The effective chlorine concentration of the final solution was determined according to the determination method of effective chlorine in the "Technical Specifications for Disinfection" (Third Edition). The specific results are shown in the following table.

[0062] Serial number Effective chlorine concentration of electrolytic hydrochloric acid (ppm) Effective chlorine concentration of electrolytic sodium chloride (ppm) Commercial Electrode 110 118 Example 1 144 131 Example 2 156 143 Example 3 142 133 Example 4 181 173

[0063] It can be seen from the above table that, compared with common commercial electrodes, using the electrode piece prepared by the present invention as an anode can greatly increase the effective chlorine concentration in the electrolytic solution.

[0064] Example 6

[0065] Taking the commercially available common ruthenium iridium titanium DSA commercial electrode as a control, the electrode pieces prepared in Examples 1-4 were taken, and the surface morphology of the electrode pieces was obtained using an optical microscope under the same magnification objective lens, as shown in FIG. Figure 1 .Depend on Figure 1 It can be seen that the surface of ordinary commercial electrodes has no obvious microporous structure. Compared with ordinary commercial electrodes, Examples 1-4 successfully construct a microporous structure on the electrode surface by adding metaaluminate and silicate to the coating liquid formula, and then using sodium hydroxide and hydrofluoric acid to remove aluminum and silicon elements, so as to achieve the rapid detachment of chlorine bubbles generated during the electrolysis process from the electrode surface, thereby improving the electrolysis efficiency. Among them, the microporous structure formed by the electrode prepared in Example 4 is the most obvious, followed by Example 2, and this result is consistent with the effective chlorine concentration data measured in Example 5.

Claims

1. A method for preparing an efficient chlorine evolution electrode, characterized in that: The specific steps are as follows: Step 1, sandblasting the surface of the titanium substrate to obtain a substrate, and cleaning and drying the substrate; Step 2, adding the noble metal salt, dispersant, stabilizer and pore-forming agent precursor into the reactor, adjusting the pH value to 5-8, the temperature to 50-65° C., and reacting for 4-6 hours to obtain a coating solution; Step 3, applying the coating liquid of step 2 to the surface of the substrate dried in step 1, and after the surface of the substrate is dried, performing high-temperature sintering, and then repeating the coating liquid application and high-temperature sintering for multiple times until a coating thickness that meets the requirements is obtained; Step 4, adding the substrate sintered and solidified in step 3 into a NaOH solution and boiling it, and then washing it with water ultrasound until the surface is free of alkalinity; Step 5, immersing the substrate treated in step 4 in hydrofluoric acid for ultrasonic reaction, and then ultrasonically cleaning with water until the surface is free of acidity; Step 6: sinter the substrate processed in step 5 again at high temperature.

2. The method for preparing a high-efficiency chlorine evolution electrode according to claim 1, characterized in that: In step 1, the substrate is cleaned by pickling with 10% oxalic acid solution at a temperature of 90-100° C. for 60-90 min. After pickling, the substrate is further cleaned by ultrasound for 20-40 min.

3. The method for preparing a high-efficiency chlorine evolution electrode according to claim 1, characterized in that: In the step 1, the drying is carried out by air drying or drying in a drying oven; the conditions for the drying in the drying oven are as follows: a drying temperature of 100 to 120° C. and a drying time of 20 to 30 minutes.

4. The method for preparing a high-efficiency chlorine evolution electrode according to claim 1, characterized in that: In the step 2, the noble metal salt is a mixture of ruthenium trichloride, tantalum pentachloride, chloroiridic acid and chloroplatinic acid.

5. The method for preparing a high-efficiency chlorine evolution electrode according to claim 1, characterized in that: In the step 2, the dispersant is one of ethanol, isopropanol or n-butanol.

6. The method for preparing a high-efficiency chlorine evolution electrode according to claim 1, characterized in that: In the step 2, the stabilizer is one of ethylene glycol, citric acid, PVP polymer, titanium tetrachloride, titanium trichloride and tetrabutyl titanate, or two of ethylene glycol, citric acid and PVP polymer.

7. The method for preparing a high-efficiency chlorine evolution electrode according to claim 1, characterized in that: In the step 2, the pore-forming agent precursor is a mixture of sodium aluminate and tetrabutyl silicate in a mass ratio of 1:1 to 5.

8. The method for preparing a high-efficiency chlorine evolution electrode according to claim 1, characterized in that: In the step 2, the ratio of the noble metal salt, the dispersant, the stabilizer and the pore former precursor by mass is 1:1-5:10-15:0.001-0.

05.

9. The method for preparing a high-efficiency chlorine evolution electrode according to claim 4, characterized in that: In the step 2, the noble metal salt is a mixture of ruthenium trichloride, tantalum pentachloride, chloroiridic acid and chloroplatinic acid in a mass ratio of 1:0.1 to 1:0.1 to 1:0.1 to 0.

5.

10. The method for preparing a high-efficiency chlorine evolution electrode according to claim 1, characterized in that: In step 3, the high temperature sintering temperature is 250-450° C., and the sintering time is 10-15 minutes.

11. The method for preparing a high-efficiency chlorine evolution electrode according to claim 1, characterized in that: In step 4, the concentration of NaOH is 40-60%wt, and the boiling time is 30-60min.

12. The method for preparing a high-efficiency chlorine evolution electrode according to claim 1, characterized in that: In step 5, the concentration of hydrofluoric acid is 10-30%wt, and the ultrasonic reaction time is 30-60min.

13. The method for preparing a high-efficiency chlorine evolution electrode according to claim 1, characterized in that: In step 6, the high temperature sintering temperature is 450-550° C., and the sintering time is 10-15 minutes.

Citation Information

Cited By

  • Intelligent temperature control and bubble elimination plasma electrode system and control method thereof

    CN119406347A

  • Intelligent temperature control and bubble elimination plasma electrode system and control method thereof

    CN119406347B