Production process of flat yarn polyester wool tops
By accurately controlling the heat setting temperature and slurrying process, the problems of unstable temperature and uneven slurrying in the production of flat silk polyester wool strips are solved, the quality and production efficiency of the product are improved, and the good heat setting and uniform coating of the fibers are ensured. .
Patent Information
- Application Number
- CN202410925317.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing flat silk polyester wool strip production process, the thermal setting temperature control range is large, resulting in unstable product quality and uneven slurry, which affects the flatness and gloss of the fibers.
By precisely controlling the heat setting temperature and speed, optimizing the concentration and speed of the slurry slurry, ensuring that the polyester wire obtains good heat setting effect during the dry tissue process and achieves uniform slurry coating.
It improves the elasticity and elongation of the fiber, ensures the controllability and stability of the weaving process, reduces product variability and defect rate, improves the overall quality and aesthetics of the product, and improves production efficiency and economic benefits.
Smart Images

Figure CN118957784A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyester top production, in particular to a production process of flat polyester top. Background Art
[0002] Flat polyester top is a fabric strip product made of polyester fiber. It has a flat shape and soft feel and is widely used in the field of textiles. Compared with traditional round fibers, flat polyester top has a larger surface area and can provide better gloss and touch. At the same time, due to the characteristics of the flat shape, flat polyester top is easier to form a flat and uniform fabric during the weaving process, and usually has good ductility, which can be used to make fabrics that require softness and stretchability. When flat polyester top is produced, the temperature of heat setting can be controlled to ensure that the polyester yarn obtains a good heat setting effect during the dry weaving process. However, in the current process, when the temperature of heat setting is controlled, the range is usually large, which results in that if the temperature is not suitable at the current heat setting speed, the product quality will be low for a long distance. Therefore, a production process of flat polyester top is proposed. Summary of the invention
[0003] In view of the shortcomings of the prior art, the present invention provides a production process for flat polyester yarn, which solves the problem that in the current process, when controlling the temperature of heat setting, the range is usually large, which leads to the problem that if the temperature is not suitable at the current heat setting speed, the product quality will be low for a long distance.
[0004] To achieve the above objectives, the present invention is implemented through the following technical solutions: A production process of flat polyester wool tops, comprising the following steps:
[0005] S1. Prepare the raw materials required for production;
[0006] S2, pre-processing the raw materials prepared in step S1;
[0007] S3, subjecting the polyester yarn initially processed in step S2 to heat setting treatment;
[0008] S4, further processing the polyester yarn after heat setting in step S3 into wool tops;
[0009] S5, rolling up the wool strips obtained in step S4 and conducting random inspection;
[0010] S6, packaging the wool strips rolled up in step S5 and sending them to a warehouse for storage.
[0011] Preferably, the raw material in step S1 is polyester raw material, and the primary processing in step S2 includes polymerization, spinning, drawing, shaping and sizing.
[0012] Preferably, the polymerization temperature is between 260° C. and 300° C., and the spinning speed is between 4200 and 5800 m / min.
[0013] Preferably, the stretching speed is between 3200-4000 m / min, and the setting temperature is between 150° C.-200° C.
[0014] Preferably, the concentration of the slurry during the slurry addition is between 0.8% and 1.4%, the pH value of the slurry during the slurry addition is between 6.4 and 7.2, and the speed during the slurry addition is between 17 and 30 m / min.
[0015] Preferably, the temperature during the heat setting treatment in step S3 is between 195° C. and 215° C., and the speed during the heat setting treatment is between 45 and 75 m / min.
[0016] Preferably, the further processing steps of the polyester yarn in step S4 include stringing and weaving, the speed of the stringing is between 170-220 m / min, the temperature of the weaving is between 45° C.-58° C., and the speed of the weaving is between 2000-3600 m / min.
[0017] Preferably, the sampling interval is between 300m and 500m, and the winding speed is between 2800 and 4000m / min.
[0018] The present invention provides a production process for flat polyester wool tops. Compared with the prior art, it has the following beneficial effects:
[0019] (1) The production process of the flat polyester sliver can ensure that the polyester filaments obtain a good heat setting effect during the dry weaving process by precisely controlling the temperature, thereby improving the elasticity and extensibility of the fibers, ensuring the weavability and processability of the fibers during the weaving process, and making the fiber surface smoother, thereby improving the appearance and glossiness of the fibers and improving the overall quality and aesthetics of the product.
[0020] (2) The production process of the flat polyester sliver can stabilize the production process and reduce fluctuations and adverse conditions in the production process by reducing the temperature variation range during the heat setting process, thereby ensuring consistent heat setting effects on the fibers, making the entire production process more controllable and stable, and reducing product variability and defective rates. Appropriate temperature control can increase the heat setting speed and efficiency of the fibers, speed up production rhythm, and increase production capacity and benefits, thereby achieving the purpose of improving product quality, stabilizing the production process, and improving production efficiency and economic benefits.
[0021] (3) The production process of the flat polyester top can ensure that the surface of the polyester yarn is evenly coated with slurry by strictly controlling the concentration and speed of slurry during slurry addition, thereby avoiding uneven slurry coating. The appropriate slurry addition speed can ensure that the polyester yarn is evenly coated within a suitable time, thereby avoiding excessive consumption of slurry. The even slurry coating helps to improve the flatness, glossiness and softness of the product, ensure the consistency and reliability of the product, and help to improve product quality while reducing waste of resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] See also Figure 1 , the present invention provides the following technical solutions:
[0025] Embodiment 1: A production process of flat polyester tops, comprising the following steps:
[0026] S1. Prepare the raw materials required for production, the raw materials are polyester raw materials;
[0027] S2, the raw materials prepared in step S1 are preliminarily processed, and the preliminarily processing steps include polymerization, spinning, drawing, shaping and slurrying, the temperature during polymerization is 260°C, the spinning speed is 4200m / min, the drawing speed is 3200m / min, the shaping temperature is 150°C, the slurry concentration during slurrying is 0.8%, the slurry pH value during slurrying is 6.4, and the slurrying speed is 17m / min;
[0028] S3, subjecting the polyester yarn after the initial processing in step S2 to heat setting treatment, the temperature during the heat setting treatment is 195° C., and the speed during the heat setting treatment is 45 m / min;
[0029] S4, further processing the polyester yarn after heat setting in step S3 into wool tops, the further processing steps of the polyester yarn include yarn stringing and weaving, the speed of yarn stringing is 170m / min, the temperature of weaving is 45°C, and the speed of weaving is 2000m / min;
[0030] S5, rolling up the wool strips obtained in step S4 and performing random inspection, the inspection interval is 300m, and the rolling speed is 2800m / min;
[0031] S6, packaging the wool strips rolled up in step S5 and sending them to a warehouse for storage.
[0032] Embodiment 2: A production process of flat polyester tops, comprising the following steps:
[0033] S1. Prepare the raw materials required for production, the raw materials are polyester raw materials;
[0034] S2, the raw materials prepared in step S1 are preliminarily processed, the preliminarily processing steps include polymerization, spinning, drawing, shaping and slurrying, the temperature during polymerization is 280°C, the spinning speed is 4400m / min, the drawing speed is 3400m / min, the shaping temperature is 160°C, the slurry concentration during slurrying is 0.9%, the slurry pH value during slurrying is 6.8, and the slurrying speed is 18m / min;
[0035] S3, subjecting the polyester yarn after the initial processing in step S2 to heat setting treatment, the temperature during the heat setting treatment is 200° C., and the speed during the heat setting treatment is 48 m / min;
[0036] S4, further processing the polyester yarn after heat setting in step S3 into wool tops, the further processing steps of the polyester yarn include yarn stringing and weaving, the speed of yarn stringing is 175m / min, the temperature of weaving is 47°C, and the speed of weaving is 2500m / min;
[0037] S5, rolling up the wool strips obtained in step S4 and performing random inspection, the inspection interval is 350m, and the rolling speed is 2900m / min;
[0038] S6, packaging the wool strips rolled up in step S5 and sending them to a warehouse for storage.
[0039] Embodiment 3: A production process of flat polyester tops, comprising the following steps:
[0040] S1. Prepare the raw materials required for production, the raw materials are polyester raw materials;
[0041] S2, the raw material prepared in step S1 is subjected to primary processing, the primary processing steps include polymerization, spinning, drawing, shaping and slurrying, the temperature during polymerization is 280°C, the spinning speed is 4500m / min, the drawing speed is 3800m / min, the shaping temperature is 170°C, the slurry concentration during slurrying is 1%, the slurry pH value during slurrying is 7, and the slurrying speed is 19m / min;
[0042] S3, subjecting the polyester yarn after the initial processing in step S2 to heat setting treatment, the temperature during the heat setting treatment is 205° C., and the speed during the heat setting treatment is 49 m / min;
[0043] S4, further processing the polyester yarn after heat setting in step S3 into wool tops, the further processing steps of the polyester yarn include yarn stringing and weaving, the speed of yarn stringing is 180m / min, the temperature of weaving is 46°C, and the speed of weaving is 2900m / min;
[0044] S5, rolling up the wool strips obtained in step S4 and performing random inspection, the inspection interval is 400m, and the rolling speed is 3000m / min;
[0045] S6, packaging the wool strips rolled up in step S5 and sending them to a warehouse for storage.
[0046] Embodiment 4: A production process of flat polyester tops, comprising the following steps:
[0047] S1. Prepare the raw materials required for production, the raw materials are polyester raw materials;
[0048] S2, the raw material prepared in step S1 is subjected to primary processing, the primary processing steps include polymerization, spinning, drawing, shaping and slurrying, the temperature during polymerization is 295°C, the spinning speed is 4800m / min, the drawing speed is 3900m / min, the shaping temperature is 185°C, the slurry concentration during slurrying is 1.2%, the slurry pH value during slurrying is 6.9, and the slurrying speed is 25m / min;
[0049] S3, subjecting the polyester yarn after the initial processing in step S2 to heat setting treatment, wherein the temperature during the heat setting treatment is 215° C. and the speed during the heat setting treatment is 60 m / min;
[0050] S4, further processing the polyester yarn after heat setting in step S3 into wool tops, the further processing steps of the polyester yarn include yarn stringing and weaving, the speed of yarn stringing is 190m / min, the temperature of weaving is 52°C, and the speed of weaving is 3300m / min;
[0051] S5, rolling up the wool strips obtained in step S4 and performing random inspection, the inspection interval is 450m, and the rolling speed is 3300m / min;
[0052] S6, packaging the wool strips rolled up in step S5 and sending them to a warehouse for storage.
[0053] Embodiment 5: A production process of flat polyester tops, comprising the following steps:
[0054] S1. Prepare the raw materials required for production, the raw materials are polyester raw materials;
[0055] S2, the raw material prepared in step S1 is subjected to primary processing, the primary processing steps include polymerization, spinning, drawing, shaping and slurrying, the temperature during polymerization is 300° C., the spinning speed is 4800 m / min, the drawing speed is 3900 m / min, the shaping temperature is 182° C., the slurry concentration during slurrying is 1.3%, the slurry pH value during slurrying is 6.9, and the slurrying speed is 29 m / min;
[0056] S3, subjecting the polyester yarn after the initial processing in step S2 to heat setting treatment, the temperature during the heat setting treatment is 214° C., and the speed during the heat setting treatment is 58 m / min;
[0057] S4, further processing the polyester yarn after heat setting in step S3 into wool tops, the further processing steps of the polyester yarn include yarn stringing and weaving, the speed of yarn stringing is 200m / min, the temperature of weaving is 46°C, and the speed of weaving is 3000m / min;
[0058] S5, rolling up the wool strips obtained in step S4 and performing random inspection, the inspection interval is 480m, and the rolling speed is 3500m / min;
[0059] S6, packaging the wool strips rolled up in step S5 and sending them to a warehouse for storage.
[0060] Embodiment 6: A production process of flat polyester tops, comprising the following steps:
[0061] S1. Prepare the raw materials required for production, the raw materials are polyester raw materials;
[0062] S2, the raw material prepared in step S1 is subjected to primary processing, the primary processing steps include polymerization, spinning, drawing, shaping and slurrying, the temperature during polymerization is 285°C, the spinning speed is 5000m / min, the drawing speed is 3400m / min, the shaping temperature is 155°C, the slurry concentration during slurrying is 1.4%, the slurry pH value during slurrying is 7.1, and the slurrying speed is 28m / min;
[0063] S3, subjecting the polyester yarn after the initial processing in step S2 to heat setting treatment, the temperature during the heat setting treatment is 213° C., and the speed during the heat setting treatment is 57 m / min;
[0064] S4, further processing the polyester yarn after heat setting in step S3 into wool tops, the further processing steps of the polyester yarn include yarn stringing and weaving, the speed of yarn stringing is 200m / min, the temperature of weaving is 46°C, and the speed of weaving is 3000m / min;
[0065] S5, rolling up the wool strips obtained in step S4 and performing random inspection, the inspection interval is 480m, and the rolling speed is 3500m / min;
[0066] S6, packaging the wool strips rolled up in step S5 and sending them to a warehouse for storage.
[0067] Embodiment 7: A production process of flat polyester tops, comprising the following steps:
[0068] S1. Prepare the raw materials required for production, the raw materials are polyester raw materials;
[0069] S2, the raw material prepared in step S1 is subjected to primary processing, the primary processing steps include polymerization, spinning, drawing, shaping and slurrying, the temperature during polymerization is 265°C, the spinning speed is 4300m / min, the drawing speed is 3400m / min, the shaping temperature is 175°C, the slurry concentration during slurrying is 0.9%, the slurry pH value during slurrying is 7.2, and the slurrying speed is 22m / min;
[0070] S3, subjecting the polyester yarn after the initial processing in step S2 to heat setting treatment, the temperature during the heat setting treatment is 212° C., and the speed during the heat setting treatment is 75 m / min;
[0071] S4, further processing the polyester yarn after heat setting in step S3 into wool tops, the further processing steps of the polyester yarn include yarn stringing and weaving, the speed of yarn stringing is 200m / min, the temperature of weaving is 46°C, and the speed of weaving is 3000m / min;
[0072] S5, rolling up the wool strips obtained in step S4 and performing random inspection, the inspection interval is 480m, and the rolling speed is 3500m / min;
[0073] S6, packaging the wool strips rolled up in step S5 and sending them to a warehouse for storage.
[0074] Embodiment 8: A production process of flat polyester tops, comprising the following steps:
[0075] S1. Prepare the raw materials required for production, the raw materials are polyester raw materials;
[0076] S2, the raw material prepared in step S1 is subjected to primary processing, the primary processing steps include polymerization, spinning, drawing, shaping and slurrying, the temperature during polymerization is 275°C, the spinning speed is 4500m / min, the drawing speed is 3800m / min, the shaping temperature is 190°C, the slurry concentration during slurrying is 0.85%, the slurry pH value during slurrying is 6.5, and the slurrying speed is 19m / min;
[0077] S3, subjecting the polyester yarn after the initial processing in step S2 to heat setting treatment, the temperature during the heat setting treatment is 211° C., and the speed during the heat setting treatment is 70 m / min;
[0078] S4, further processing the polyester yarn after heat setting in step S3 into wool tops, the further processing steps of the polyester yarn include stringing and weaving, the speed of the stringing is 200m / min, the temperature of the weaving is 46°C, and the speed of the weaving is 3300m / min;
[0079] S5, rolling up the wool strips obtained in step S4 and performing random inspection, the inspection interval is 380m, and the rolling speed is 3000m / min;
[0080] S6, packaging the wool strips rolled up in step S5 and sending them to a warehouse for storage.
[0081] Embodiment 9: A production process of flat polyester tops, comprising the following steps:
[0082] S1. Prepare the raw materials required for production, the raw materials are polyester raw materials;
[0083] S2, the raw material prepared in step S1 is subjected to primary processing, the primary processing steps include polymerization, spinning, drawing, shaping and slurrying, the temperature during polymerization is 275°C, the spinning speed is 4500m / min, the drawing speed is 3800m / min, the shaping temperature is 190°C, the slurry concentration during slurrying is 0.85%, the slurry pH value during slurrying is 6.5, and the slurrying speed is 19m / min;
[0084] S3, subjecting the polyester yarn after the initial processing in step S2 to heat setting treatment, the temperature during the heat setting treatment is 209° C., and the speed during the heat setting treatment is 68 m / min;
[0085] S4, further processing the polyester yarn after heat setting in step S3 into wool tops, the further processing steps of the polyester yarn include stringing and weaving, the speed of the stringing is 200m / min, the temperature of the weaving is 46°C, and the speed of the weaving is 3300m / min;
[0086] S5, rolling up the wool strips obtained in step S4 and performing random inspection, the inspection interval is 380m, and the rolling speed is 3000m / min;
[0087] S6, packaging the wool strips rolled up in step S5 and sending them to a warehouse for storage.
[0088] Embodiment 10: A production process of flat polyester tops, comprising the following steps:
[0089] S1. Prepare the raw materials required for production, the raw materials are polyester raw materials;
[0090] S2, the raw materials prepared in step S1 are preliminarily processed, and the preliminarily processing steps include polymerization, spinning, drawing, shaping and slurrying, the temperature during polymerization is 30°C, the spinning speed is 5800m / min, the drawing speed is 4000m / min, the shaping temperature is 200°C, the slurry concentration during slurrying is 0.95%, the slurry pH value during slurrying is 6.6, and the slurrying speed is 30m / min;
[0091] S3, subjecting the polyester yarn after the initial processing in step S2 to heat setting treatment, the temperature during the heat setting treatment is 204° C., and the speed during the heat setting treatment is 63 m / min;
[0092] S4, further processing the polyester yarn after heat setting in step S3 into wool tops, the further processing steps of the polyester yarn include yarn stringing and weaving, the speed of yarn stringing is 220m / min, the temperature of weaving is 58°C, and the speed of weaving is 3600m / min;
[0093] S5, rolling up the wool strips obtained in step S4 and performing random inspection, the inspection interval is 500m, and the rolling speed is 4000m / min;
[0094] S6, packaging the wool strips rolled up in step S5 and sending them to a warehouse for storage.
[0095] After the production according to the above embodiment, the optimal heat setting temperature is 190°C; the optimal heat setting speed is 68m / min; the optimal slurry concentration is 0.95%; and the optimal slurry adding speed is 22m / min.
[0096] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.
[0097] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0098] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A production process for flat polyester tops, characterized in that: The following steps are involved: S1. Prepare the raw materials required for production; S2, pre-processing the raw materials prepared in step S1; S3, subjecting the polyester yarn initially processed in step S2 to heat setting treatment; S4, further processing the polyester yarn after heat setting in step S3 into wool tops; S5, rolling up the wool strips obtained in step S4 and conducting random inspection; S6, packaging the wool strips rolled up in step S5 and sending them to a warehouse for storage.
2. The process for producing flat polyester tops according to claim 1, characterized in that: The raw material in step S1 is polyester raw material, and the primary processing in step S2 includes polymerization, spinning, drawing, shaping and sizing.
3. The process for producing flat polyester tops according to claim 2, characterized in that: The polymerization temperature is between 260° C. and 300° C., and the spinning speed is between 4200 and 5800 m / min.
4. The process for producing flat polyester tops according to claim 2, characterized in that: The drawing speed is between 3200-4000 m / min, and the setting temperature is between 150° C.-200° C.
5. The process for producing flat polyester tops according to claim 2, characterized in that: The concentration of the slurry during the slurry addition is between 0.8% and 1.4%, the pH value of the slurry during the slurry addition is between 6.4 and 7.2, and the speed during the slurry addition is between 17 and 30 m / min.
6. The process for producing flat polyester tops according to claim 1, characterized in that: The temperature during the heat setting treatment in step S3 is between 175° C. and 235° C., and the speed during the heat setting treatment is between 45 and 75 m / min.
7. The process for producing flat polyester tops according to claim 1, characterized in that: In step S4, the further processing steps of the polyester yarn include stringing and weaving, the speed of the stringing is between 170-220 m / min, the temperature of the weaving is between 45° C.-58° C., and the speed of the weaving is between 2000-3600 m / min.
8. The process for producing flat polyester tops according to claim 1, characterized in that: The sampling inspection interval is between 300m and 500m, and the winding speed is between 2800 and 4000m / min.