Long and deep concrete crack treatment process for bridge and culvert thin-wall platform

By opening grooves along the cracks on the thin-walled platform of the bridge and culvert, filling phosphate cement, filling epoxy resin and covering and coating, the water leakage and steel bar corrosion caused by concrete cracks are solved, extending the service life of the bridge and culvert and improving the stability.

CN118958179APending Publication Date: 2024-11-15ROAD & BRIDGE INT CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411228936.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the construction process, the concrete surface cracks often occur in the thin-walled platform of the bridge and culvert often lead to serious crack development, resulting in water leakage and premature rust of the steel bars, shortening the service life of the structure.

Method used

Use a cutting mechanism to open grooves along the cracks in depth and width. After removing the dust, fill the phosphate cement slurry, drill holes and fill the epoxy resin slurry, and seal and cover and brush after curing.

Benefits of technology

Effectively treat concrete cracks, extend the service life of the structure, and improve functional stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118958179A_ABST
    Figure CN118958179A_ABST
Patent Text Reader

Abstract

The invention discloses a long and deep concrete crack treatment process for a bridge and culvert thin-wall platform. The long and deep concrete crack treatment process comprises the following steps that a cutting mechanism is used for forming equal-depth and equal-width grooves along the path where a crack is located; floating dust in the groove is removed through compressed air; a seam sealing material is blended, and the groove after floating dust removal is fully embedded; after the seam sealing material is cured, sealing inspection and repairing are conducted; holes penetrating through the crack are drilled in the positions, corresponding to the two sides of the crack groove respectively; epoxy resin slurry is poured into the crack positions through the holes; after the epoxy resin slurry is initially set, the holes are blocked; and epoxy putty is used for covering and brushing along the crack and the two sides of the crack. The technical problems that in the prior art, the concrete crack treatment process is not ideal, crack development is more and more serious, water leakage occurs or steel bars are corroded too early, and then the service life of a structure is shortened are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bridge and culvert engineering construction, and in particular to a long and deep concrete crack treatment process for a thin-wall platform of a bridge and culvert. Background Art

[0002] At present, in the construction process of thin-walled abutments of bridges and culverts, the problem of concrete surface cracking often occurs. After analysis, there are two main reasons for the above problem:

[0003] 1. The platform body has large components and dense reinforcement, which leads to a long time for concrete pouring, resulting in a time interval between the upper and lower layers of concrete pouring;

[0004] 2. When workers are pouring concrete for the platform, the main reinforcement or formwork shakes, causing internal disturbance of the concrete and cracking.

[0005] In the prior art, concrete cracks are often not handled in a timely or ideal manner, resulting in increasingly serious crack development, and then problems such as water leakage or premature corrosion of steel bars, which seriously shortens the service life of the structure. Summary of the invention

[0006] To this end, the present invention provides a long and deep concrete crack treatment process for thin-walled platforms of bridges and culverts, so as to solve the technical problem in the prior art that the concrete crack treatment process is not ideal, resulting in increasingly serious crack development, water leakage or premature rusting of steel bars, thereby shortening the service life of the structure.

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] A long and deep concrete crack treatment process for thin-walled abutments of bridges and culverts comprises the following steps:

[0009] Use a cutting mechanism to create grooves of equal depth and width along the path of the crack;

[0010] Use compressed air to remove floating dust inside the groove;

[0011] Mix the sealing material and fill the grooves after removing the dust;

[0012] After the sealing material is solidified, check and repair the seal;

[0013] Drill holes through the cracks at two sides of the crack groove;

[0014] Inject epoxy resin slurry into the crack position through the holes;

[0015] After the epoxy resin slurry has initially solidified, the holes are sealed;

[0016] Use epoxy putty to cover the crack and its sides.

[0017] On the basis of the above technical solution, the present invention is further described as follows:

[0018] As a further embodiment of the present invention,

[0019] The method of using a cutting mechanism to open grooves of equal depth and width along the path of the crack specifically includes:

[0020] Use a cutting mechanism to create grooves of equal depth and width along the path of the crack;

[0021] The width of the grooves of equal depth and width shall not be less than 1.5 cm, and the depth shall not be less than 2 cm.

[0022] As a further embodiment of the present invention,

[0023] The mixing of the sealing material and filling the grooves after removing the floating dust specifically includes:

[0024] Phosphate cement slurry with a dry mix ratio of 7:2.5 is used as a sealing material, and the grooves after removing the dust are filled with the phosphate cement slurry, and then the phosphate cement slurry is smoothed.

[0025] As a further embodiment of the present invention,

[0026] The holes corresponding to the two sides of the crack groove are drilled through the cracks, specifically including:

[0027] Continue to drill holes on both sides of the groove corresponding to the crack, and keep the holes on both sides of the groove cross-set, the spacing of the holes on each side along the crack extension path is set to 0.2-0.3m, and the directions of the holes are inclined through the cracks, so as to be used as grouting holes or exhaust holes;

[0028] Each crack is connected to at least one grouting hole and one exhaust hole.

[0029] As a further embodiment of the present invention,

[0030] The spacing of the holes on each side along the crack extension path is set to 0.2-0.3m, specifically including:

[0031] According to the principle that the narrower the crack, the smaller the hole spacing, when the crack width is in the range of 0.2mm to 0.3mm, the spacing of the holes along the crack extension path is set to 0.2m, and when the crack width is in the range of 0.3mm to 0.4mm, the spacing of the holes along the crack extension path is set to 0.3m.

[0032] As a further embodiment of the present invention,

[0033] The method of injecting epoxy resin slurry into the crack position through the holes specifically includes:

[0034] Use a high-pressure injection machine to inject epoxy resin slurry into the crack position through the injection holes;

[0035] The mixing ratio of the epoxy resin slurry is set to epoxy resin: dibutyl phthalate: ethylenediamine (industrial): xylene (industrial) = 100: 10: 8-11: 30-40;

[0036] Among them, the epoxy resin uses bisphenol A type E-44 (601#), the epoxy value is 0.41-0.42, the industrial ethylenediamine content is more than 70%, and the epoxy resin density is 1062kg / m 3 .

[0037] As a further embodiment of the present invention,

[0038] The method of pouring epoxy resin slurry into the crack position through the holes specifically includes:

[0039] Before starting grouting, conduct a ventilation test, open all valves of the pipeline between the high-pressure grouting machine and the grouting nozzle to connect the pipeline, and use compressed air with a pressure of more than 0.2MPa to purge the pipeline and cracks. When sweeping the effective cracks, the compressed air is transferred from the grouting hole through the cracks to the exhaust hole for discharge;

[0040] The purpose of the ventilation test is to understand whether the injection holes and cracks are unobstructed and to check whether the edge sealing is effective, so as to determine whether the glue can be injected; specifically, when compressed air is filled into the cracks, observe but not limited to the unobstructed condition of each hole, whether the sealed edge seams are leaking, and whether there are air leaks in the surrounding concrete;

[0041] Afterwards, based on the grouting sequence from top to bottom, grouting was carried out continuously along the drilled holes. The grouting pressure range was maintained at 0.2-0.4MPa, and the pressure increased gradually to prevent sudden pressurization from causing the cracks to expand.

[0042] As a further embodiment of the present invention,

[0043] The operation steps of pouring epoxy resin slurry specifically include:

[0044] Open all valves of the pipeline between the high-pressure grouting machine and the grouting nozzle to connect the pipeline;

[0045] Inject the prepared epoxy resin slurry into the high-pressure injection machine;

[0046] Open the gas cylinder valve corresponding to the high-pressure grouting machine and adjust the grouting pressure range to 0.2-0.4MPa;

[0047] Open the valve leading to the grouting nozzle of the grouting tank corresponding to the high-pressure grouting machine;

[0048] Start grouting, and perform the grouting process in the holes drilled on one side of the crack extension path in sequence. When grout emerges from the intersecting adjacent holes, close the valve of the current grouting nozzle, and continue grouting in sequence until the grouting rate at the final position reaches 0.1L / min. After maintaining the pressure for 5 to 10 minutes, stop the grouting process corresponding to the crack and close the corresponding grouting nozzle valve;

[0049] Conduct core sampling and / or open hole endoscopy at crack locations where grouting is performed.

[0050] As a further embodiment of the present invention,

[0051] After the epoxy resin slurry is initially solidified, the holes are blocked, which specifically includes:

[0052] After the epoxy resin slurry in the cracks has initially solidified, use sealing glue to seal, smooth and clean the surfaces of the holes and openings formed by core sampling and / or endoscopic inspection;

[0053] The use of epoxy putty to cover and paint along the crack and both sides thereof specifically includes:

[0054] Use epoxy putty to apply 2 coats along the crack and 10cm on both sides;

[0055] The mixing ratio of epoxy putty is set to epoxy resin: dibutyl phthalate: ethylenediamine (industrial): xylene (industrial): cement = 100: 10: 13-15: 20: 250-450;

[0056] Among them, the epoxy resin uses bisphenol A type E-44 (601#), the epoxy value is 0.41~0.42, the cement grade is 325# or above, the industrial ethylenediamine content is above 70%, and the epoxy putty density is 1121k / m 3 .

[0057] As a further solution of the present invention, the following steps are also included:

[0058] Carry out surface color treatment on the painted parts;

[0059] Continuously observe the generation and treatment of the crack;

[0060] The surface color treatment of the painted part specifically includes:

[0061] Use sandpaper to sand the epoxy putty coating area corresponding to the cracks in the order of coarse and fine to a smooth base surface, then use a vacuum cleaner to remove all dust from the base surface, and then fine-tune the color difference agent according to the established color difference, and then apply the color difference agent to the base surface of the concrete component, and apply it at least twice;

[0062] The continuous observation of the generation and treatment of the crack specifically includes:

[0063] First, observe whether the cracks after treatment continue to develop;

[0064] The second is to observe whether the treatment part is in a stable state.

[0065] The present invention has the following beneficial effects:

[0066] This treatment process can carry out deep treatment of concrete cracks and fine surface modification, which can effectively solve the crack defects of concrete, thereby ensuring the service life of the structure and improving functional stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0067] In order to more clearly illustrate the implementation mode of the present invention or the technical solution in the prior art, the drawings required for the implementation mode or the description of the prior art will be briefly introduced below. The structures, proportions, sizes, etc. illustrated in this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read. Any structural modification, change in proportional relationship or adjustment of size should still fall within the scope of the technical contents disclosed in the present invention without affecting the effects and purposes that can be achieved by the present invention.

[0068] Figure 1 A schematic flow chart of an overall method for treating long and deep concrete cracks in thin-walled abutments of bridges and culverts provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0069] The following is a description of the implementation of the present invention by specific embodiments. People familiar with the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0070] The terms such as "upper", "lower", "left", "right", and "middle" used in this specification are only for the convenience of description and are not intended to limit the scope of the invention. Changes or adjustments to their relative relationships should be regarded as within the scope of the invention without substantially changing the technical content.

[0071] like Figure 1 As shown, an embodiment of the present invention provides a long and deep concrete crack treatment process for a thin-walled platform of a bridge culvert, comprising the following steps:

[0072] S1: Use a cutting mechanism to create grooves of equal depth and width along the crack path;

[0073] The specific process is: use a cutting mechanism to open grooves of equal depth and width along the path of the crack, and the width of the grooves of equal depth and width is not less than 1.5 cm, and the depth is not less than 2 cm.

[0074] S2: Use compressed air to remove floating dust inside the groove;

[0075] The specific process is: use compressed air with a pressure of more than 0.2MPa to remove floating dust inside the groove.

[0076] S3: Mix the sealing material and fill the grooves after removing the dust;

[0077] The specific process is: mix phosphate cement slurry with a dry mix ratio of 7:2.5 as the sealing material, and use the phosphate cement slurry to fill the grooves after removing the dust, and then grind the phosphate cement slurry flat;

[0078] S4: Wait for the sealing material to solidify, then perform sealing inspection and repair;

[0079] The specific process is as follows: after the phosphate cement slurry solidifies, a layer of soapy water is applied along the edge seams formed by the phosphate cement slurry, and compressed air with a pressure of 0.2MPa is introduced along the edge seams to check the sealing effect of the edge seams. The air leakage parts where bubbles are generated by the soapy water are sealed with phosphate cement slurry;

[0080] S5: holes are drilled through the cracks at both sides of the crack groove;

[0081] The specific process is as follows: holes are drilled on both sides of the groove corresponding to the crack, and the holes on both sides of the groove are arranged crosswise, the spacing of the holes on each side along the crack extension path is set to 0.2-0.3m, and the directions of the holes are inclined to pass through the cracks, so as to be used as grouting holes or exhaust holes;

[0082] Each crack has at least one corresponding grouting hole and one exhaust hole;

[0083] An optional implementation scheme, according to the epoxy resin glue-in characteristics and construction experience, if a satisfactory grouting effect is to be achieved, the smaller the hole spacing should be, the easier it is to block the narrower the crack is. When the crack width is in the range of 0.2mm to 0.3mm, the spacing of the holes along the crack extension path is set to 0.2m; when the crack width is in the range of 0.3mm to 0.4mm, the spacing of the holes along the crack extension path is set to 0.3m;

[0084] S6: injecting epoxy resin slurry into the crack position through the holes;

[0085] The specific process is: use a high-pressure injection machine to inject epoxy resin slurry into the crack position through the injection hole;

[0086] The mixing ratio of the epoxy resin slurry is set to epoxy resin: dibutyl phthalate: ethylenediamine (industrial): xylene (industrial) = 100: 10: 8-11: 30-40;

[0087] Among them, the epoxy resin uses bisphenol A type E-44 (601#), the epoxy value is 0.41-0.42, the industrial ethylenediamine content is more than 70%, and the epoxy resin density is 1062kg / m 3 ;

[0088] More specifically, a ventilation test is conducted before starting grouting. All valves of the pipeline between the high-pressure grouting machine and the grouting nozzle are opened to connect the pipeline. Compressed air with a pressure of more than 0.2MPa is used to purge the pipeline and cracks. When the effective cracks are purged, the compressed air is transferred from the grouting hole through the crack to the exhaust hole for discharge.

[0089] The purpose of the ventilation test is to understand whether the injection holes and cracks are unobstructed and to check whether the edge sealing is effective, so as to determine whether the glue can be injected; specifically, when compressed air is filled into the cracks, observe but not limited to the unobstructed condition of each hole, whether the sealed edge seams are leaking, and whether there are air leaks in the surrounding concrete;

[0090] Afterwards, based on the grouting sequence from top to bottom, grouting was carried out continuously along the drilled holes. The grouting pressure range was maintained at 0.2-0.4 MPa, and the pressure was gradually increased to prevent the cracks from expanding due to sudden pressure increase.

[0091] More specifically, the operation steps of pouring epoxy resin slurry include the following process:

[0092] S601: Open all valves of the pipeline between the high-pressure grouting machine and the grouting nozzle to connect the pipeline;

[0093] S602: injecting the prepared epoxy resin slurry into a high-pressure injection machine;

[0094] S603: Open the valve of the gas cylinder corresponding to the high-pressure grouting machine and adjust the grouting pressure range to maintain at 0.2-0.4 MPa;

[0095] S604: Open the valve leading to the grouting nozzle of the grouting tank corresponding to the high-pressure grouting machine;

[0096] S605: start grouting, and perform grouting process in order along the holes drilled on one side of the crack extension path. When grouting occurs in the intersecting adjacent holes, close the valve of the current grouting nozzle, and continue grouting in order until the grouting rate at the final position reaches 0.1L / min. After the pressure is maintained for 5 to 10 minutes, stop the grouting process corresponding to the crack, and close the grouting nozzle valve.

[0097] Carry out core sampling and / or perforated endoscope inspection at the crack locations where grouting is to be performed to effectively ensure the quality of grouting sealing;

[0098] S7: After the epoxy resin slurry is initially solidified, the holes are sealed;

[0099] The specific process is as follows: after the epoxy resin slurry inside the crack has initially solidified, each hole and the opening formed by core sampling and / or endoscopic inspection are sealed, smoothed and the surface cleaned with sealing glue;

[0100] S8: Use epoxy putty to cover the crack and its two sides;

[0101] The specific process is: use epoxy putty to apply 2 coats along the crack and its two sides, 10 cm each;

[0102] The mixing ratio of epoxy putty is set to epoxy resin: dibutyl phthalate: ethylenediamine (industrial): xylene (industrial): cement = 100: 10: 13-15: 20: 250-450;

[0103] Among them, the epoxy resin uses bisphenol A type E-44 (601#), the epoxy value is 0.41~0.42, the cement grade is 325# or above, the industrial ethylenediamine content is above 70%, and the epoxy putty density is 1121k / m 3 ;

[0104] S9: Perform surface color treatment on the painted area;

[0105] The specific process is: use sandpaper to grind the epoxy putty painting range corresponding to the cracks in the order of coarse and fine to a smooth base surface, then use a vacuum cleaner to remove all dust from the base surface, and then fine-tune the color difference agent according to the established color difference, and then apply the color difference agent to the base surface of the concrete component, and apply it at least twice;

[0106] S10: Continuously observe the generation and treatment of the crack;

[0107] The specific process is: first, observe whether the cracks after treatment continue to develop;

[0108] The second is to observe whether the treatment part is in a stable state.

[0109] Although the present invention has been described in detail above by general description and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements can be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all belong to the scope of protection claimed by the present invention.

Claims

1. A process for treating long and deep concrete cracks in thin-walled abutments of bridges and culverts, characterized in that: The steps include: Use a cutting mechanism to create grooves of equal depth and width along the path of the crack; Use compressed air to remove floating dust inside the groove; Mix the sealing material and fill the grooves after removing the dust; After the sealing material is solidified, check and repair the seal; Drill holes through the cracks at two sides of the crack groove; Inject epoxy resin slurry into the crack position through the holes; After the epoxy resin slurry has initially solidified, the holes are sealed; Use epoxy putty to cover the crack and its sides.

2. The long and deep concrete crack treatment process for thin-walled abutments of bridges and culverts according to claim 1 is characterized in that: The method of using a cutting mechanism to open grooves of equal depth and width along the path of the crack specifically includes: Use a cutting mechanism to create grooves of equal depth and width along the path of the crack; The width of the grooves of equal depth and width shall not be less than 1.5 cm, and the depth shall not be less than 2 cm.

3. The long and deep concrete crack treatment process for thin-walled abutments of bridges and culverts according to claim 2 is characterized in that: The mixing of the sealing material and filling the grooves after removing the floating dust specifically includes: Phosphate cement slurry with a dry mix ratio of 7:2.5 is used as a sealing material, and the grooves after removing the dust are filled with the phosphate cement slurry, and then the phosphate cement slurry is smoothed.

4. The long and deep concrete crack treatment process for thin-walled abutments of bridges and culverts according to claim 3 is characterized in that: The holes corresponding to the two sides of the crack groove are drilled through the cracks, specifically including: Continue to drill holes on both sides of the groove corresponding to the crack, and keep the holes on both sides of the groove cross-set, the spacing of the holes on each side along the crack extension path is set to 0.2-0.3m, and the directions of the holes are inclined through the cracks, so as to be used as grouting holes or exhaust holes; Each crack is connected to at least one grouting hole and one exhaust hole.

5. The long and deep concrete crack treatment process for thin-walled abutments of bridges and culverts according to claim 4 is characterized in that: The spacing of the holes on each side along the crack extension path is set to 0.2-0.3m, specifically including: According to the principle that the narrower the crack, the smaller the hole spacing, when the crack width is in the range of 0.2mm to 0.3mm, the spacing of the holes along the crack extension path is set to 0.2m, and when the crack width is in the range of 0.3mm to 0.4mm, the spacing of the holes along the crack extension path is set to 0.3m.

6. The long and deep concrete crack treatment process for thin-walled abutments of bridges and culverts according to claim 5 is characterized in that: The method of injecting epoxy resin slurry into the crack position through the holes specifically includes: Use a high-pressure injection machine to inject epoxy resin slurry into the crack position through the injection holes; The mixing ratio of the epoxy resin slurry is set to epoxy resin: dibutyl phthalate: ethylenediamine (industrial): xylene (industrial) = 100: 10: 8-11: 30-40; Among them, the epoxy resin uses bisphenol A type E-44 (601#), the epoxy value is 0.41-0.42, the industrial ethylenediamine content is more than 70%, and the epoxy resin density is 1062kg / m 3 .

7. The long and deep concrete crack treatment process for thin-walled abutments of bridges and culverts according to claim 6 is characterized in that: The method of pouring epoxy resin slurry into the crack position through the holes specifically includes: Before starting grouting, conduct a ventilation test, open all valves of the pipeline between the high-pressure grouting machine and the grouting nozzle to connect the pipeline, and use compressed air with a pressure of more than 0.2MPa to purge the pipeline and cracks. When sweeping the effective cracks, the compressed air is transferred from the grouting hole through the cracks to the exhaust hole for discharge; The purpose of the ventilation test is to understand whether the injection holes and cracks are unobstructed and to check whether the edge sealing is effective, so as to determine whether the glue can be injected; specifically, when compressed air is filled into the cracks, observe but not limited to the unobstructed condition of each hole, whether the sealed edge seams are leaking, and whether there are air leaks in the surrounding concrete; Afterwards, based on the grouting sequence from top to bottom, grouting was carried out continuously along the drilled holes. The grouting pressure range was maintained at 0.2-0.4MPa, and the pressure increased gradually to prevent sudden pressurization from causing the cracks to expand.

8. The long and deep concrete crack treatment process for thin-walled abutments of bridges and culverts according to claim 7 is characterized in that: The operation steps of pouring epoxy resin slurry specifically include: Open all valves of the pipeline between the high-pressure grouting machine and the grouting nozzle to connect the pipeline; Inject the prepared epoxy resin slurry into the high-pressure injection machine; Open the gas cylinder valve corresponding to the high-pressure grouting machine and adjust the grouting pressure range to 0.2-0.4MPa; Open the valve leading to the grouting nozzle of the grouting tank corresponding to the high-pressure grouting machine; Start grouting, and perform the grouting process in the holes drilled on one side of the crack extension path in sequence. When grout emerges from the intersecting adjacent holes, close the valve of the current grouting nozzle, and continue grouting in sequence until the grouting rate at the final position reaches 0.1L / min. After maintaining the pressure for 5 to 10 minutes, stop the grouting process corresponding to the crack and close the corresponding grouting nozzle valve; Conduct core sampling and / or open hole endoscopy at crack locations where grouting is performed.

9. The long and deep concrete crack treatment process for thin-walled abutments of bridges and culverts according to claim 8 is characterized in that: After the epoxy resin slurry is initially solidified, the holes are blocked, which specifically includes: After the epoxy resin slurry in the cracks has initially solidified, use sealing glue to seal, smooth and clean the surface of each hole and the opening formed by core sampling and / or endoscopic inspection; The use of epoxy putty to cover and paint along the crack and both sides thereof specifically includes: Use epoxy putty to apply 2 coats along the crack and 10cm on both sides; The mixing ratio of epoxy putty is set to epoxy resin: dibutyl phthalate: ethylenediamine (industrial): xylene (industrial): cement = 100: 10: 13-15: 20: 250-450; Among them, the epoxy resin uses bisphenol A type E-44 (601#), the epoxy value is 0.41~0.42, the cement grade is 325# or above, the industrial ethylenediamine content is above 70%, and the epoxy putty density is 1121k / m 3 .

10. The long and deep concrete crack treatment process for thin-walled abutments of bridges and culverts according to claim 9 is characterized in that: The following steps are also included: Carry out surface color treatment on the painted parts; Continuously observe the generation and treatment of the crack; The surface color treatment of the painted part specifically includes: Use sandpaper to sand the epoxy putty coating area corresponding to the cracks in the order of coarse and fine to a smooth base surface, then use a vacuum cleaner to remove all dust from the base surface, and then fine-tune the color difference agent according to the established color difference, and then apply the color difference agent to the base surface of the concrete component, and apply it at least twice; The continuous observation of the generation and treatment of the crack specifically includes: First, observe whether the cracks after treatment continue to develop; The second is to observe whether the treatment part is in a stable state.