Method for testing coating compactness of silver-coated nickel powder

The nickel ion content is determined by reacting sulfuric acid and hydrogen peroxide with nickel peroxide and combining with titration method, which solves the problem that the coating density of nickel permeable powder in the prior art cannot be quantitatively analyzed, and provides a simple and effective The test method evaluates the density of the silver cladding and improves the conductivity and oxidation resistance.

CN118961994AInactive Publication Date: 2024-11-15SUZHOU XINGHAN NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411014491.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to quantitatively analyze the density of the silver cladding layer in the nickel silver-clad powder, resulting in a decrease in the conductivity in a high temperature and high humidity environment, and there is a lack of effective detection methods.

Method used

The content of nickel ions was measured by titration method, and the density of the silver-clad cladding layer was indirectly evaluated, using ammonium purpurine urea as an indicator, combined with ethylenediamine Titration was performed on the standard solution of disodium tetraacetate to calculate the amount of exposed nickel in the nickel-clad powder.

Benefits of technology

It provides a test method that is simple to operate, small sample quantity and good repeatability, can quantitatively analyze the density of the silver cladding layer, and is suitable for lateral comparison between different samples, effectively assessing conductivity and oxidation resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004965314260000021
    Figure BDA0004965314260000021
  • Figure BDA0004965314260000041
    Figure BDA0004965314260000041
  • Figure BDA0004965314260000051
    Figure BDA0004965314260000051
Patent Text Reader

Abstract

The invention relates to the technical field of metal powder material detection, in particular to a method for testing the coating compactness of silver-coated nickel powder, which comprises the following steps: mixing the silver-coated nickel powder with a dilute sulfuric acid solution and a hydrogen peroxide solution to obtain a mixed solution; centrifuging the mixed solution, taking supernate, adding deionized water, an ammonium chloride buffer solution and a violuric acid ammonium indicator, and uniformly mixing to obtain a solution to be detected; titrating the to-be-detected solution by using a disodium ethylene diamine tetraacetate standard solution until the to-be-detected solution becomes purple, recording the volume of the disodium ethylene diamine tetraacetate standard solution consumed by titration, and calculating the content of nickel exposed on the surface layer in the silver-coated nickel powder according to a formula. The test method provided by the invention is simple and convenient to operate, small in sample consumption and good in repeatability, can quantitatively analyze the compactness of the silver coating layer, has transverse contrast for the compactness of the silver coating layers of different samples, and can solve the technical problem that the coating compactness of the silver-coated nickel powder cannot be quantitatively analyzed in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal powder material detection, in particular to a method for testing the coating density of silver-coated nickel powder. Background Art

[0002] Silver powder is widely used in the field of electronic pastes because of its relatively stable physical and chemical properties, excellent electrical conductivity, and good thermal conductivity. In order to reduce manufacturing costs, using low-priced metals such as copper and nickel to replace precious metals to make conductor pastes and conductive coatings is an important trend in the future development of electronic industry materials. At present, the application of silver-coated nickel powder in low-temperature polymer conductor pastes can reduce production costs by 2 / 3.

[0003] As a filling material for conductive paste, silver-coated nickel powder must have good anti-oxidation properties to ensure the reliability of silver-coated nickel powder after curing and to pass high temperature and high humidity tests after being made into components. Zhou Dongxiang et al. mentioned in "Study on the Anti-oxidation of Ultrafine Nickel-Silver Bimetallic Powder [J]. Electronic Components and Materials, 2007, 26 (3): 15-17" that a layer of nanosilver was coated on the surface of submicron nickel powder to make nickel-silver bimetallic powder by liquid phase chemical reduction method. The effects of silver content and nickel powder particle size on the coating effect and the anti-oxidation property of bimetallic powder were studied. Li Shudong et al. mentioned in "Coating Structure and Anti-oxidation Property of Micron Nickel-Silver Bimetallic Powder [J]. Rare Metal Materials and Engineering, 2006, 35 (5): 817-819" that the anti-oxidation ability of nickel-silver bimetallic powder is related to the surface coating structure and the surface silver content of the particles. The higher the silver content, the tighter the surface coating and the higher the anti-oxidation temperature. However, if the coating density of silver-coated nickel is low, even if the silver content is high, the exposed nickel element outside the silver-coated nickel powder can easily react with oxygen in the air to form a nickel oxide layer, resulting in a significant decrease in conductivity and even problems in high temperature and high humidity tests of the components.

[0004] At present, the research focus of silver plating on nickel powder surface is on the preparation method and process optimization, while there are few reports on the in-depth research on the coating density of silver-coated nickel powder. Therefore, designing a quantitative analysis method to detect the density of the silver coating layer in silver-coated nickel powder has become an urgent problem to be solved in this field. Summary of the invention

[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for testing the coating density of silver-coated nickel powders. Sulfuric acid and hydrogen peroxide react with the nickel exposed on the surface of the silver-coated nickel powders. Due to the different densities of the silver coating, the contact area between the solution and the nickel is different, and the degree of corrosion to the nickel is also different. The present invention samples and analyzes the content of nickel ions at the same time point. The resistance value is low, indicating excellent conductivity, and the titrated nickel content is low, indicating that the density of the silver coating layer is good. The test method for the coating density of the silver-coated nickel powder provided by the present invention is simple and convenient to operate, with a small amount of sample and good repeatability. The density of the silver coating layer can be quantitatively analyzed, and the density of the silver coating layer between different samples has lateral comparison, which can effectively solve the technical problem that the coating density of the silver-coated nickel powder cannot be quantitatively analyzed in the prior art.

[0006] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0007] The present invention provides a method for testing the coating density of silver-coated nickel powder, comprising the following steps:

[0008] (1) mixing silver-coated nickel powder with a dilute sulfuric acid solution and a hydrogen peroxide solution to obtain a mixed solution;

[0009] (2) centrifuging the mixed solution described in step (1), taking the supernatant, adding deionized water, ammonium chloride buffer and murexide indicator, and mixing evenly to obtain a test solution;

[0010] (3) titrating the test solution in step (2) with a disodium ethylenediaminetetraacetic acid standard solution until it turns purple, and recording the volume of the disodium ethylenediaminetetraacetic acid standard solution consumed in the titration;

[0011] (4) Calculate the nickel content exposed on the surface of the silver-coated nickel powder according to the following formula:

[0012]

[0013] Where:

[0014] c: free nickel content, unit: mol / L;

[0015] C 1 : Concentration of disodium EDTA standard solution, unit: mol / L;

[0016] V 1 : The volume of disodium EDTA standard solution consumed in titration, unit: mL;

[0017] V: volume of the supernatant of the mixed solution, unit: mL.

[0018] Furthermore, the steps of preparing the mixed solution in step (1) include:

[0019] (A) Weigh 2 g of silver-coated nickel powder and place it in a 50 mL centrifuge tube;

[0020] (B) Add 30 g of dilute sulfuric acid solution and 800 μL of hydrogen peroxide solution to a centrifuge tube;

[0021] (C) placing the centrifuge tube in an oscillator for oscillation to obtain the mixed solution.

[0022] Further, the mass fraction of the dilute sulfuric acid solution is 3% to 20%, and illustratively, the mass fraction of the dilute sulfuric acid solution is 3%, 10.7% or 20%. Preferably, the mass fraction of the dilute sulfuric acid solution is 3%.

[0023] Further, the mass fraction of the hydrogen peroxide solution is 20% to 30%, and illustratively, the mass fraction of the hydrogen peroxide solution is 20%, 25% or 30%. Preferably, the mass fraction of the hydrogen peroxide solution is 20%.

[0024] Further, the frequency of the oscillator is 300 r / min, and the oscillation time is 3 to 120 min. For example, the oscillation time is 3 min, 5 min, 15 min, 30 min, 60 min, 90 min or 120 min. Preferably, the oscillation time is 5 min.

[0025] Furthermore, the preparation step of the test solution in step (2) includes:

[0026] (A) centrifuging the mixed solution with a centrifuge and taking the supernatant for later use;

[0027] (B) Measure 20 mL of the supernatant of the mixed solution and add it to a 250 mL conical flask;

[0028] (C) Add 50 mL of deionized water, 19 mL of ammonium chloride buffer, and 0.01 g of murexide indicator to a conical flask and mix until the solution turns bright yellow.

[0029] Furthermore, the centrifugal frequency of the centrifuge is 6000 rpm.

[0030] Further, the titration process in step (3) comprises the following steps:

[0031] (A) Add 10 mL of disodium EDTA standard solution into the burette;

[0032] (B) titrating the test solution with the disodium ethylenediaminetetraacetic acid standard solution in step (A) until the test solution turns purple, and the titration endpoint is reached when the color does not return to the original color after shaking for 30 seconds;

[0033] (C) Record the volume of disodium EDTA standard solution consumed in the titration.

[0034] Furthermore, the concentration of the disodium ethylenediaminetetraacetic acid standard solution is 0.05 mol / L.

[0035] The present invention has the following beneficial effects:

[0036] The present invention uses ammonium murexate as an indicator and uses EDTA standard solution to perform complex titration on the nickel ion content, thereby indirectly characterizing the compactness of the silver coating layer in the silver-coated nickel powder. According to the reaction of sulfuric acid and hydrogen peroxide with the nickel exposed on the surface of the silver-coated nickel powder, the chemical reaction formula is: Ni+H 2 O 2 +2H + =Ni 2+ +2H 2 O, due to the different compactness of silver coating, the different exposed nickel content, the different contact areas between solution and nickel, and the different degrees of corrosion to nickel, the nickel ion content measured by titration can reflect the degree of nickel corrosion, and then reflect the compactness of silver coating. By sampling and analyzing the content of nickel ions at the same time point, the resistance value is low, indicating excellent conductivity, and the titrated nickel content is low, indicating that the compactness of the silver coating is good, otherwise it is the opposite. The test method provided by the present invention is simple to operate, has a small amount of sample, and has good stability. It can quantitatively analyze the compactness of the powder silver coating, and has a horizontal comparative test method for the compactness of the silver coating between different samples. DETAILED DESCRIPTION

[0037] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, it does not mean that the features of this invention are limited to the implementation.

[0038] Reagent Preparation:

[0039] (1) 0.05 mol / L EDTA disodium standard solution: accurately weigh 16.81 g of EDTA solid and dissolve it in deionized water. Stir thoroughly until it becomes colorless and transparent, and then dilute to 1000 mL for later use.

[0040] (2) 0.02 mol / L potassium permanganate solution, used to calibrate hydrogen peroxide solution. Preparation method: Accurately weigh 1.571 g of potassium permanganate solid and dissolve it in deionized water, and dilute to 500 mL for later use.

[0041] (3) Dilute sulfuric acid solution

[0042] 1) 20% sulfuric acid solution, preparation method: 360mL deionized water and 50mL concentrated sulfuric acid, stir evenly, and set aside;

[0043] 2) 10.7% sulfuric acid solution, preparation method: 300mL deionized water and 20mL concentrated sulfuric acid, stir evenly, and set aside;

[0044] 3) 3% sulfuric acid solution, preparation method: 500mL deionized water and 9mL concentrated sulfuric acid, stir and dissolve until transparent, set aside.

[0045] (4) Hydrogen peroxide solution

[0046] 1) 30% hydrogen peroxide solution, a common commercial reagent;

[0047] 2) 20% hydrogen peroxide solution: accurately weigh 50g of 30% hydrogen peroxide solution and 25g of deionized water, mix them thoroughly, put them in a brown reagent bottle, and place them in a cool and dark place for use.

[0048] Wherein, the calibration of 20% hydrogen peroxide solution includes the following steps:

[0049] ① Accurately weigh 0.32 g of the above-prepared 20% hydrogen peroxide solution (error ≤ 0.001), and weigh 200 mL of the above-prepared 10.7% dilute sulfuric acid solution;

[0050] ② Add 20% hydrogen peroxide solution to 10.7% dilute sulfuric acid solution and shake evenly;

[0051] ③ Add 0.02 mol / L of the prepared potassium permanganate solution into the burette to the 50 mL mark;

[0052] ④ Use the potassium permanganate solution from step ③ to start titrating the mixed liquid from step ②. Stop titrating when the color of the solution changes from colorless and transparent to lavender, and the titration is completed when there is no color change after shaking for 30 seconds.

[0053] ⑤ Calculate the content of hydrogen peroxide solution according to the following formula:

[0054]

[0055] In the above formula:

[0056] w: content of hydrogen peroxide solution (unit: %);

[0057] V: the amount of potassium permanganate titrated (unit: mL);

[0058] C: concentration of potassium permanganate (unit: 0.02 mol / L);

[0059] M: molecular weight of hydrogen peroxide (unit: 34.01 g / mol);

[0060] m: weight of hydrogen peroxide (unit: g).

[0061] ⑥ Calculate the hydrogen peroxide concentration according to step ⑤. It can be used normally if the concentration is between 19% and 21%.

[0062] (6) Ammonia-ammonium chloride buffer (pH=10), preparation method: 50 g of ammonium chloride solid and 500 mL of deionized water were mixed and stirred to dissolve until colorless and transparent, and then 300 mL of ammonia water was added and stirred until a colorless and transparent solution was obtained.

[0063] (7) Ammonium murexate indicator.

[0064] Example:

[0065] A method for testing the coating density of silver-coated nickel powder, specifically comprising the following steps:

[0066] (1) Accurately weigh 2.00 g of sample (error ≤ 0.001) and place it in a clean 50 mL centrifuge tube;

[0067] (2) adding 30 g of a 3% to 20% by mass dilute sulfuric acid solution and 800 μL of a 20% to 30% by mass hydrogen peroxide solution to the above centrifuge tubes, respectively, covering the tubes, and vibrating the tubes on an oscillator to obtain a mixed solution;

[0068] (3) The oscillator frequency is 300 r / min, and the oscillation time is 5 min. After the oscillation is completed, the centrifuge tube is quickly taken out and placed in a centrifuge for centrifugation (pay attention to balancing). The centrifugation frequency reaches 6000 rpm. The above process needs to be completed quickly. After centrifugation, pour out the supernatant into a new centrifuge tube;

[0069] (4) Use a pipette to accurately measure 20 mL of the supernatant (volume V) of the mixed solution in step (3) into a 250 mL conical flask, add 50 mL of deionized water to the conical flask, then use a dispenser to add 19 mL of ammonium chloride buffer, and add 0.01 g of murexide indicator and shake evenly until the solution turns bright yellow, thereby obtaining a test solution;

[0070] (5) Pour a 0.05 mol / L disodium ethylenediaminetetraacetic acid standard solution (concentration C1) into a burette to a scale of 10 mL, and use the burette to titrate the test solution in step (4) at a low speed. Stop the titration when the solution turns purple. Shake for 30 seconds and the color does not return to its original color, which is the titration endpoint. Record the volume of the disodium ethylenediaminetetraacetic acid standard solution consumed in the titration (volume V1).

[0071] (6) Calculation of titration results:

[0072]

[0073] Where:

[0074] c: free nickel content, unit: mol / L;

[0075] C 1 : Concentration of disodium EDTA standard solution, unit: mol / L;

[0076] V 1 : The volume of disodium EDTA standard solution consumed in titration, unit: mL;

[0077] V: volume of the supernatant of the mixed solution removed, unit: mL.

[0078] The present invention uses sulfuric acid and hydrogen peroxide to react with nickel exposed on the surface. Due to the different compactness of the silver coating, the contact surface size of the solution and the nickel is different, and the degree of corrosion of the nickel is also different. By sampling and analyzing the content of nickel ions at the same time point, the resistance value is low, indicating excellent conductivity, and the titrated nickel content is low, indicating that the compactness of the silver coating layer is good. The test method provided by the present invention is simple and fast in test operation, uses less sample, and has good stability.

[0079] In order to make the purpose, technical scheme and advantages of the present invention clearer, the embodiments of the present invention are further described in detail below. In the following examples, unless otherwise specified, the raw materials used are all common commercially available products, and the silver-coated nickel powder used is selected from the silver-coated nickel powder of Suzhou Xinghan New Material Technology Co., Ltd.

[0080] Example 1

[0081] This embodiment provides a method for testing the coating density of silver-coated nickel powder, comprising the following steps:

[0082] (1) Accurately weigh 2.00 g (error ≤ 0.001) of silver-coated nickel powder and add it to a clean 50 mL centrifuge tube;

[0083] (2) Add 30 g of 3% by mass dilute sulfuric acid solution and 800 μL of 20% by mass hydrogen peroxide solution to the above centrifuge tube, cover the tube, and place it on an oscillator for vibration and mixing to obtain a mixed solution; wherein the oscillator frequency is 300 r / min and the oscillation time is 3 min;

[0084] (3) After the shaking is completed, quickly take out the centrifuge tube and place it on the centrifuge for centrifugation (pay attention to the balance), and the centrifugal speed reaches 6000 rpm. The above process needs to be completed quickly. After centrifugation, take the supernatant in the centrifuge tube and put it into a new centrifuge tube for standby use;

[0085] (4) Use a pipette to accurately measure 20 mL of the supernatant of the mixed solution and add it to a 250 mL conical flask, and add 50 mL of deionized water to the conical flask and shake it evenly; use a dispenser to add 19 mL of ammonium chloride buffer and 0.01 g of murexide indicator to the conical flask, shake it evenly, and the solution turns bright yellow to obtain a test solution;

[0086] (5) Pour a 0.05 mol / L disodium ethylenediaminetetraacetic acid standard solution into a burette to a scale of 10 mL, and titrate the test solution at a low speed with the 0.05 mol / L disodium ethylenediaminetetraacetic acid standard solution until the test solution turns purple. The titration endpoint is reached if the solution does not return to its original color after shaking for 30 s. Record the volume of the 0.05 mol / L disodium ethylenediaminetetraacetic acid standard solution consumed in the titration.

[0087] (6) The oscillation time of the mixed solution was adjusted to 5 min, 15 min, 30 min, 60 min, 90 min, and 120 min, respectively, and the above steps (1) to (5) were repeated in sequence.

[0088] In this embodiment, three different silver-coated nickel powder samples 1-3 are used, and the above steps (1)-(6) are repeated in sequence. The titration results of each group of samples are shown in Table 1.

[0089] Table 1 Relationship between titration nickel content and reaction time

[0090]

[0091] Analysis of the data in Table 1 above shows that, for the same silver-coated nickel powder sample, extending the reaction time can increase the free nickel ion content; for different silver-coated nickel powder samples, when sampling at the same time point, the lower the resistance value of the sample, the better its conductivity, and the lower the titrated nickel content, the better the density of its silver coating layer. Considering the reaction effect and time cost, the reaction time of 5 min can be used as a reference standard for the following experiments to further optimize the experimental parameters.

[0092] Example 2

[0093] This embodiment provides a method for testing the coating density of silver-coated nickel powder, comprising the following steps:

[0094] (1) Accurately weigh 2.00 g (error ≤ 0.001) of silver-coated nickel powder and add it to a clean 50 mL centrifuge tube;

[0095] (2) Add 30 g of a 3% by mass dilute sulfuric acid solution and 800 μL of a 30% by mass hydrogen peroxide solution to the above centrifuge tube, cover the tube with a lid, and place the tube on an oscillator for vibrating and mixing to obtain a mixed solution; wherein the oscillator frequency is 300 r / min and the oscillation time is 5 min;

[0096] (3) After the shaking is completed, quickly take out the centrifuge tube and place it on the centrifuge for centrifugation (pay attention to the balance), and the centrifugal speed reaches 6000 rpm. The above process needs to be completed quickly. After centrifugation, take the supernatant in the centrifuge tube and put it into a new centrifuge tube for standby use;

[0097] (4) Use a pipette to accurately measure 20 mL of the supernatant of the mixed solution and add it to a 250 mL conical flask, and add 50 mL of deionized water to the conical flask and shake it evenly; use a dispenser to add 19 mL of ammonium chloride buffer and 0.01 g of murexide indicator to the conical flask, shake it evenly, and the solution turns bright yellow to obtain a test solution;

[0098] (5) Pour 0.05 mol / L EDTA standard solution into a burette to the mark of 10 mL. Titrate the test solution with the 0.05 mol / L EDTA standard solution at a low speed until the test solution turns purple. The titration endpoint is when the color does not return to its original color after shaking for 30 s. Record the volume of the 0.05 mol / L EDTA standard solution consumed in the titration.

[0099] In this embodiment, three different silver-coated nickel powder samples 1 to 3 are used, and the above steps (1) to (5) are repeated in sequence. The titration results of each group of samples are shown in Table 2.

[0100] Table 2 Relationship between titration nickel content and hydrogen peroxide concentration

[0101]

[0102] Analysis of the data in Table 2 shows that for the same silver-coated nickel powder sample, the nickel ion content is analyzed under the conditions of the same reaction time and the same sulfuric acid concentration. As the hydrogen peroxide concentration increases, the titration result of the nickel content increases slightly, and the change is not obvious. Considering cost savings, 20% concentration hydrogen peroxide can be preferably used for the test.

[0103] Example 3

[0104] This embodiment provides a method for testing the coating density of silver-coated nickel powder, comprising the following steps:

[0105] (1) Accurately weigh 2.00 g (error ≤ 0.001) of silver-coated nickel powder and add it to a clean 50 mL centrifuge tube;

[0106] (2) Add 30 g of 10.7% by mass dilute sulfuric acid solution and 800 μL of 20% by mass hydrogen peroxide solution to the above centrifuge tube, cover the tube with a lid, and place the tube on an oscillator for vibration and mixing to obtain a mixed solution; wherein the oscillator frequency is 300 r / min and the oscillation time is 5 min;

[0107] (3) After the shaking is completed, quickly take out the centrifuge tube and place it on the centrifuge for centrifugation (pay attention to the balance), and the centrifugal speed reaches 6000 rpm. The above process needs to be completed quickly. After centrifugation, take the supernatant in the centrifuge tube and put it into a new centrifuge tube for standby use;

[0108] (4) Use a pipette to accurately measure 20 mL of the supernatant of the mixed solution and add it to a 250 mL conical flask, and add 50 mL of deionized water to the conical flask and shake it evenly; use a dispenser to add 19 mL of ammonium chloride buffer and 0.01 g of murexide indicator to the conical flask, shake it evenly, and the solution turns bright yellow to obtain a test solution;

[0109] (5) Pour a 0.05 mol / L disodium ethylenediaminetetraacetic acid standard solution into a burette to a scale of 10 mL, and titrate the test solution at a low speed with the 0.05 mol / L disodium ethylenediaminetetraacetic acid standard solution until the test solution turns purple. The titration endpoint is reached if the solution does not return to its original color after shaking for 30 s. Record the volume of the 0.05 mol / L disodium ethylenediaminetetraacetic acid standard solution consumed in the titration.

[0110] (6) The mass fraction of the dilute sulfuric acid solution in step (2) is adjusted to 20%, and the above steps (1) to (5) are repeated in sequence.

[0111] In this embodiment, three different silver-coated nickel powder samples 1 to 3 are used, and the above steps (1) to (6) are repeated in sequence. The titration results of each group of samples are shown in Table 3.

[0112] Table 3 Relationship between titration nickel content and sulfuric acid concentration

[0113]

[0114] Analysis of the data in Table 3 above shows that for the same silver-coated nickel powder sample, the nickel ion content is analyzed under the conditions of sampling at the same time point and the same hydrogen peroxide concentration. As the sulfuric acid concentration increases, the titration result of the nickel content increases, but the change is not obvious. Considering cost savings, sulfuric acid with a mass fraction of 3% can be preferably used for the test.

[0115] Comparative Example

[0116] Silver powder (resistance of 27.65 μΩ·cm) and self-synthesized nickel powder (resistance of 26343 μΩ·cm) made by Suzhou Xinghan New Material Technology Co., Ltd. were used for control test under the above optimized conditions, which specifically includes the following steps:

[0117] (1) Accurately weigh 2.00 g (error ≤ 0.001) of silver powder and add it to a clean 50 mL centrifuge tube;

[0118] (2) Add 30 g of 3% by mass dilute sulfuric acid solution and 800 μL of 20% by mass hydrogen peroxide solution to the above centrifuge tube, cover the tube, and place it on an oscillator for vibration and mixing to obtain a mixed solution; wherein the oscillator frequency is 300 r / min and the oscillation time is 5 min;

[0119] (3) After the shaking is completed, quickly take out the centrifuge tube and place it on the centrifuge for centrifugation (pay attention to the balance), and the centrifugal speed reaches 6000 rpm. The above process needs to be completed quickly. After centrifugation, take the supernatant in the centrifuge tube and put it into a new centrifuge tube for standby use;

[0120] (4) Use a pipette to accurately measure 20 mL of the supernatant of the mixed solution and add it to a 250 mL conical flask, and add 50 mL of deionized water to the conical flask and shake it evenly; use a dispenser to add 19 mL of ammonium chloride buffer and 0.01 g of murexide indicator to the conical flask, shake it evenly, and the solution turns bright yellow to obtain a test solution;

[0121] (5) Pour a 0.05 mol / L disodium ethylenediaminetetraacetic acid standard solution into a burette to a scale of 10 mL, and titrate the test solution at a low speed with the 0.05 mol / L disodium ethylenediaminetetraacetic acid standard solution until the test solution turns purple. The titration endpoint is reached if the solution does not return to its original color after shaking for 30 s. Record the volume of the 0.05 mol / L disodium ethylenediaminetetraacetic acid standard solution consumed in the titration.

[0122] (6) Replace the silver powder in step (1) with self-compounded nickel powder, and repeat the above steps (1) to (5) in sequence.

[0123] The titration data of the comparative example and the silver-coated nickel powder in the above embodiment under the same experimental conditions are compared, and the control data are shown in Table 4.

[0124] Table 4 Data comparison of different samples under the same experimental conditions

[0125] sample Resistivity (μΩ·cm) Oxidation resistance (μΩ·cm) Nickel content (mol / L) Sample 1 68.4 113.8 0.0016 Sample 2 578 805 0.0035 Sample 3 2879 5812 0.0062 Silver powder 27.65 / 0 Self-alloyed nickel powder 26343 58411 0.1830

[0126] Comparing the data in Table 4 above, it can be seen that due to the different densities of the silver coating, the exposed nickel content is different. When the density is good, less nickel is exposed, and the nickel ion amount measured by titration is low, otherwise it is the opposite. The present invention measures the exposed nickel content in the silver-coated nickel powder by chemical titration, and can indirectly quantitatively analyze the density of the silver coating layer in the silver-coated nickel powder.

[0127] Although the preferred embodiments of the present invention have been disclosed as above, they are not intended to limit the present invention. Any person skilled in the art may make possible changes and modifications to the technical solutions of the present invention by using the methods and technical contents disclosed above without departing from the spirit and scope of the present invention. Therefore, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the contents of the technical solutions of the present invention shall fall within the protection scope of the technical solutions of the present invention.

Claims

1. A method for testing the coating density of silver-coated nickel powder, characterized in that: The following steps are involved: (1) mixing silver-coated nickel powder with a dilute sulfuric acid solution and a hydrogen peroxide solution to obtain a mixed solution; (2) centrifuging the mixed solution described in step (1), taking the supernatant, adding deionized water, ammonium chloride buffer and murexide indicator, and mixing evenly to obtain a test solution; (3) titrating the test solution in step (2) with a disodium ethylenediaminetetraacetic acid standard solution until it turns purple, and recording the volume of the disodium ethylenediaminetetraacetic acid standard solution consumed in the titration; (4) Calculate the nickel content exposed on the surface of the silver-coated nickel powder according to the following formula: Where: c: free nickel content, unit: mol / L; C1: concentration of disodium EDTA standard solution, unit: mol / L; V1: volume of disodium EDTA standard solution consumed in titration, unit: mL; V: volume of the supernatant of the mixed solution, unit: mL.

2. The method for testing the coating density of silver-coated nickel powder according to claim 1, characterized in that: The steps of preparing the mixed solution in step (1) include: (A) Weigh 2 g of silver-coated nickel powder and place it in a 50 mL centrifuge tube; (B) Add 30 g of dilute sulfuric acid solution and 800 μL of hydrogen peroxide solution to a centrifuge tube; (C) placing the centrifuge tube in an oscillator for oscillation to obtain the mixed solution.

3. The method for testing the coating density of silver-coated nickel powder according to claim 2, characterized in that: The mass fraction of the dilute sulfuric acid solution is 3% to 20%.

4. The method for testing the coating density of silver-coated nickel powder according to claim 2, characterized in that: The mass fraction of the hydrogen peroxide solution is 20% to 30%.

5. The method for testing the coating density of silver-coated nickel powder according to claim 2, characterized in that: The frequency of the oscillator is 300 r / min, and the oscillation time is 3 to 120 min.

6. The method for testing the coating density of silver-coated nickel powder according to claim 1, characterized in that: The steps of preparing the test solution in step (2) include: (A) centrifuging the mixed solution and taking the supernatant for later use; (B) Measure 20 mL of the supernatant of the mixed solution and add it to a 250 mL conical flask; (C) Add 50 mL of deionized water, 19 mL of ammonium chloride buffer, and 0.01 g of murexide indicator to a conical flask and mix until the solution turns bright yellow.

7. The method for testing the coating density of silver-coated nickel powder according to claim 6, characterized in that: The centrifugal frequency of the centrifuge is 6000 rpm.

8. The method for testing the coating density of silver-coated nickel powder according to claim 1, characterized in that: The titration process in step (3) comprises the following steps: (A) Add 10 mL of disodium EDTA standard solution into the burette; (B) titrating the test solution with the disodium ethylenediaminetetraacetic acid standard solution in step (A) until the test solution turns purple, and the titration endpoint is reached when the color does not return to the original color after shaking for 30 seconds; (C) Record the volume of disodium EDTA standard solution consumed in the titration.

9. The method for testing the coating density of silver-coated nickel powder according to claim 8, characterized in that: The concentration of the disodium ethylenediaminetetraacetic acid standard solution is 0.05 mol / L.

Citation Information

Patent Citations

  • Calibration method for concentration of EDTA standard solution and application thereof

    CN108362822A

  • Titrimetric analysis method for copper and nickel in pyrophosphate-citrate copper-nickel alloy plating solution

    CN110702845A

  • Method for measuring content of nickel and cobalt in nickel-cobalt mixed salt

    CN114397400A

  • Silver-coated copper powder, preparation method, application of silver-coated copper powder in silver-coated copper slurry and method for detecting compactness of silver coating layer in silver-coated copper powder

    CN115805310A

  • Method for measuring content of silver in silver-coated copper conductive paste by chemical titration method

    CN118191217A

Cited By

  • Silver-coated nickel paste and preparation method thereof, and metallization method of high-temperature sintered crystalline silicon solar cell

    CN119626626A

  • Detection method and detection device for copper-coated particles

    CN122016853A

  • Silver-coated nickel paste, preparation method thereof, and high-temperature sintering metallization method for crystalline silicon solar cells

    EP4790727A1