Terminal electrode silver paste for chip inductor and preparation method of terminal electrode silver paste

By using the composite technology of sheet-shaped glass powder and ultra-fine silver powder in the end electrode silver paste of the patch inductor, combined with the organic carrier, the problems of uneven fineness and insufficient adhesion of the end electrode silver paste are solved, and the patch is improved The adhesion and reliability of the inductors and reduce production costs.

CN118969352APending Publication Date: 2024-11-15ZHEJIANG ZHONGXI ELECTRONICS TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410854460.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the fineness of the silver paste at the end of the chip inductor electrode is uneven, resulting in weak adhesion, affecting the performance and reliability of the electrode.

Method used

The end electrode silver paste containing sheet glass powder is used to improve the adhesion and welding reliability of the silver layer by combining ultrafine silver powder with a specific proportion of sheet glass powder, and an organic carrier of resin and diluent.

Benefits of technology

Effectively promote the formation of silver bumps, improve welding adhesion, reduce production costs, and improve the adhesion and reliability of chip inductors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969352A_ABST
    Figure CN118969352A_ABST
Patent Text Reader

Abstract

The invention provides terminal electrode silver paste for a chip inductor. The terminal electrode silver paste comprises silver powder, flaky glass powder and an organic carrier, the particle size D50 of the flaky glass powder is 0.5-10 [mu] m, and the diameter / thickness ratio is 2-20. The end electrode silver paste is prepared by adopting the flaky glass powder with controllable size and morphology, the method has the advantages in the aspects of reducing the melting point of the glass powder, sinking after sintering of a glass body and the like, can effectively promote the formation of silver bulges of an end silver layer in the end electrode, and is of great significance in preparing a chip inductor with high adhesive force and high reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electrode materials for passive electronic components, and in particular relates to a terminal electrode silver paste for a patch inductor and a preparation method thereof. Background Art

[0002] Chip inductors, also known as power inductors, are mainly composed of ferrite cores and copper wires. Their main function is to achieve filtering, isolation, voltage regulation, biasing and other functions of electrical signals in the circuit. They are widely used in various wireless communications, automotive electronics, and household appliances. Chip inductors mainly include four types: winding type, laminated type, braided type, and film type. Among them, winding type and laminated type chip inductors are the most commonly used. The ferrite core in the winding type chip inductor is made by pressing and high-temperature sintering of ferrite powder. Laminated inductors are made using multi-layer printing technology and laminated production processes, and are smaller in size.

[0003] The terminal electrodes of the chip inductor are ferrite core, Ag layer, Ni layer and Sn layer from inside to outside. Among them, the ferrite core is a metal oxide material with ferromagnetism, which has the characteristics of high resistance, high dielectric constant and high magnetic permeability. It is usually composed of iron oxide (Fe2O3) and other metal oxides, such as manganese ferrite (MnO·Fe2O3), zinc ferrite (ZnO·Fe2O3), nickel zinc ferrite (Ni-Zn·Fe2O4) and other multi-component ferrites. The Ag layer plated on the end surface of the ferrite core is prepared by dipping, pad printing, screen printing, baking or sintering the end electrode silver paste. The Ni layer and Sn layer are made by electroplating on the basis of the silver-plated ferrite core.

[0004] As an important basic material for preparing chip inductors, the terminal electrode silver paste mainly includes ultrafine silver powder, glass powder, resin, solvent and additives. Among them, glass powder plays an important role in the terminal electrode silver paste, which can enhance adhesion, adjust viscosity, improve mechanical strength and adjust sintering performance, thereby ensuring the performance and stability of the electrode. In the selection of glass powder, it is necessary to have excellent matching with other materials in terms of crystal structure, thermal expansion coefficient, etc., and should have a low melting point and excellent adhesion. At the same time, since the subsequent production process of the terminal electrode also includes electroplating Ni and Sn metal layers, the electroplating solution used in its production process is generally acidic, so the glass powder should also have good acid resistance. Based on this, the commonly used glass powders mainly include SiO2-B2O3-Al2O3 system and Bi2O3-B2O3-Al2O3 system.

[0005] However, glass powder is generally prepared through processes such as melting, grinding or air flow crushing, and usually presents irregular particles, and the particle size and morphology are difficult to control. Larger particles in the glass powder will directly affect the fineness of the slurry and the flatness of the printed surface, which will weaken the adhesion of the terminal electrode of the chip inductor. Therefore, it is of great significance to select a glass powder with suitable size and morphology, high matching, high adhesion, low melting point and good acid resistance for the terminal electrode silver paste and the chip inductor. Summary of the invention

[0006] In order to solve the problems of uneven fineness of terminal electrode silver paste and weak adhesion of chip inductor terminal electrodes in the prior art, the present invention provides a terminal electrode silver paste containing flaky glass powder and a preparation method thereof. The use of flaky glass powder effectively improves the adhesion and reliability of the chip inductor terminal electrodes.

[0007] The technical solution adopted by the present invention is: a terminal electrode silver paste for a patch inductor, the terminal electrode silver paste comprises silver powder, flaky glass powder, and an organic carrier; the particle size D of the flaky glass powder is 50 It is 0.5 to 10 μm, and the diameter / thickness ratio is 2 to 20.

[0008] The terminal electrode silver paste for chip inductors provided by the present invention (referred to as "terminal silver paste") uses ultrafine silver powder and flaky glass powder as powder materials, and a mixed solution of resin, diluent, and additive as an organic carrier. Since the particle size of the powder in the slurry has an important influence on the fineness of the slurry and the flatness of the printed surface, and directly affects the adhesion of the terminal electrode, the present invention explores the particle fineness and morphology of silver powder and glass powder.

[0009] The terminal electrode silver paste provided by the present invention uses glass powder whose main components are SiO2-B2O3-Al2O3, and whose morphology is flaky. Experiments have shown that the use of flaky glass powder can effectively promote the formation of silver protrusions in the terminal electrode silver layer, and can also make the sintered glass body easier to sink, thereby improving the welding adhesion of the terminal electrode, which is of great significance for the preparation of high-reliability chip inductors. Furthermore, the present invention continues to compound two flaky glass powders with different particle sizes in a specific proportion. Specifically, the flaky glass powder may include a first flaky glass powder and a second flaky glass powder; the particle size D of the first flaky glass powder is 50 The particle size D of the second flake glass powder is 1 to 5 μm; 50is 0.5-2.5μm; the mass ratio of the first flaky glass powder to the second flaky glass powder is (0.8-1.2):1. Experiments have shown that compared with flaky glass powder of a single particle size, the compounded flaky glass powder can further promote the sinking of the glass body after sintering, and has a better bonding effect with the silver protrusions, which is beneficial to the improvement of the adhesion of the terminal electrode. The experiment also found that when the proportion of glass powder is equivalent, the compounded flaky glass powder can also help improve the adhesion of the terminal electrode made of low silver content (silver content less than 60%) terminal silver paste, which plays a role in reducing costs and increasing efficiency in the production of chip inductors. In addition, other metal oxides can be introduced in the process of glass powder production to further improve performance, such as one or more of K2O, Na2O, TiO2, MgO, CaO, CuO, ZnO, and V2O5.

[0010] The terminal electrode silver paste provided by the present invention uses ultrafine silver powder composed of micron / submicron silver powder in microcrystalline form, which can be synthesized by wet chemical method, and has a small particle size and a relatively uniform particle size distribution. 50 Less than 3μm. The experiment found that different particle sizes D 50 The first silver powder (D 50 =1~3μm)、the second silver powder (D 50 =0.2-1 μm) in a specific ratio, it is helpful for the silver powder to sinter at a relatively low temperature (500-700°C) to form a conductive path, and the formed silver layer and the glass body are more firmly embedded. Preferably, the silver powder includes a first silver powder and a second silver powder; the particle size D of the first silver powder is 50 The particle size D of the second silver powder is 1 to 3 μm; 50 is 0.2-1 μm; the mass ratio of the first silver powder to the second silver powder is (8-20):1.

[0011] The terminal electrode silver paste provided by the present invention uses a mixed liquid of resin, diluent and auxiliary agent as an organic carrier, which gives the silver paste fluidity, so that the terminal electrode silver paste meets the process requirements of pad printing, dip coating, screen printing and the like. Among them, the resin can be selected from at least one of ethyl cellulose, cellulose acetate butyrate, and polyvinyl butyral. High boiling point solvents such as diethylene glycol butyl ether acetate (BCA), diethylene glycol ethyl ether acetate (DCAC), dibasic acid esters (DBE), pinene alcohol, etc. are all excellent diluents. In the preparation of the terminal electrode silver paste, generally, the polymer resin and the diluent are first mixed, stirred and heated in a specific mass ratio to prepare a resin solution. In order to further improve the performance of the slurry, auxiliary agents can generally be added to the prepared resin solution. Common auxiliary agents include dispersants, leveling agents, defoamers, antioxidants and thickeners, etc., to obtain an organic carrier.

[0012] In a preferred embodiment, the terminal electrode silver paste includes 40-80wt% silver powder, 2-20wt% flaky glass powder, 2-20wt% resin, 10-50wt% diluent, and 0.1-3wt% auxiliary agent.

[0013] In a preferred embodiment, the terminal electrode silver paste comprises 30-78wt% of first silver powder, 2-10wt% of second silver powder, 1-10wt% of first flake glass powder, 1-10wt% of second flake glass powder, 2-20wt% of resin, 10-50wt% of diluent, and 0.1-3wt% of additive; the particle size D of the first silver powder is 50 The particle size D of the second silver powder is 1 to 3 μm. 50 The particle size D of the first flake glass powder is 0.2 to 1 μm; 50 The particle size D of the second flake glass powder is 1 to 5 μm. 50 0.5~2.5μm.

[0014] The present invention also provides a method for preparing the terminal electrode silver paste, the method comprising the following steps:

[0015] Step 1: Mix the resin and the diluent, heat until completely dissolved, and cool to room temperature; add the additive, mix to obtain an organic carrier; Step 2: Add flaky glass powder to the organic carrier, mix to obtain glass paste;

[0016] Step 3: Add silver powder to the glass paste, mix and roll the paste to obtain the terminal electrode silver paste.

[0017] The prepared terminal electrode silver paste is sealed after being subjected to centrifugal degassing treatment.

[0018] The present invention also provides a chip inductor, which is prepared using the terminal electrode silver paste. The preparation method of the chip inductor includes: arranging the terminal electrode silver paste at the terminal electrode of the ferrite core by dip coating, pad printing or screen printing, obtaining a terminal silver layer after heat treatment, and electroplating a nickel layer and a tin layer on the terminal silver layer in sequence to obtain the chip inductor; the heat treatment includes: drying at 100-120°C for 15-20 minutes and then sintering at 650-700°C for 15-20 minutes. In this way, the electrode side of the chip inductor forms a structure of ferrite core / terminal silver layer / nickel layer / tin layer from the inside to the outside.

[0019] Beneficial effects of the present invention:

[0020] The present invention uses flaky glass powder with controllable size and morphology to prepare terminal electrode silver paste, which has advantages in reducing the melting point of glass powder and the sinking of glass body after sintering, and can effectively promote the formation of silver protrusions in the terminal silver layer in the terminal electrode, which is of great significance for the preparation of high adhesion and high reliability chip inductors. Furthermore, the present invention also compounds two flaky glass powders with different particle sizes in a specific proportion. Experiments have shown that compared with flaky glass powders with a single particle size, the compounded flaky glass powder can also promote the low silver content (silver content less than 60%) terminal electrode silver paste to form a terminal silver layer with better adhesion, which is of great significance for reducing the production cost of terminal electrode silver paste and chip inductors. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 1 and 2 are scanning electron microscope (SEM) images of the first glass powder and the second glass powder used in Examples 1 to 4 and the irregular granular glass powder used in Comparative Example 1.

[0022] Figure 2 The scanning electron microscope (SEM) images of the silver layer of the electrode end after sintering of Examples 1 to 4 and Comparative Example 1 are shown, wherein (a) to (d) correspond to Examples 1 to 4 respectively, and (e) corresponds to Comparative Example 1. DETAILED DESCRIPTION

[0023] The following is an explanation of the embodiments of the present invention by specific specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied by other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that, in the absence of conflict, the features in the following embodiments and embodiments can be combined with each other. In the embodiments of the present invention, the methods used are all conventional methods unless otherwise specified, and the reagents used can be obtained from commercial sources.

[0024] In the embodiment of the present invention, two kinds of silver powder are selected, namely the first silver powder and the second silver powder, and the specific specifications are as follows:

[0025] First silver powder: particle size D 50 =1.442μm, particle size D 90 =2.386μm, specific surface area 1.278m 2 / g;

[0026] Second silver powder: particle size D 50 =0.694μm, particle size D 90 =1.568μm, specific surface area 2.908m 2 / g.

[0027] In the embodiments of the present invention, the present invention mainly adopts flaky glass powder to prepare silver paste for inductor terminal electrodes, and its main component is SiO2-Al2O3-B2O3. In the embodiments, the first glass powder (#1 glass powder, with a diameter-thickness ratio of about 5.32) and the second glass powder (#2 glass powder, with a diameter-thickness ratio of about 6.65) with flaky morphology but different diameter-thickness ratios are respectively selected, or the first glass powder and the second glass powder are mixed for use. Comparative Example 1 selects the conventionally used irregular granular glass powder (#3 glass powder). The above three glass powders are tested respectively, and their composition, morphology and particle size information are shown in Table 1. Figure 1 Scanning electron microscope (SEM) images of three glass powders.

[0028] Table 1. Composition, morphology and particle size information of glass powder

[0029] serial number Glass powder name Morphology <![CDATA[Particle size D 50 > <![CDATA[Particle size D 90 > Diameter-thickness ratio #1 First glass powder Flake 1.809μm 5.201μm 5.32 #2 Second glass powder Flake 0.973μm 3.726μm 6.65 #3 Granular glass powder Irregular granular 5.642μm 14.04μm /

[0030] Note: The diameter-to-thickness ratio is the ratio of the average particle size of the flaky glass powder to its average thickness.

[0031] Examples 1 to 4 and Comparative Example 1:

[0032] In Examples 1 to 4 and Comparative Example 1, terminal electrode silver paste for chip inductors is prepared according to the specific formulas provided in Table 2, and the prepared terminal electrode silver paste is dip-coated on the ferrite core electrode, and a terminal silver layer is obtained after heat treatment. A nickel layer and a tin layer are electroplated on the terminal silver layer in sequence, thereby forming a ferrite / terminal silver / nickel / tin structure from the inside to the outside on the electrode side to obtain a chip inductor.

[0033] In terms of formula, Example 1 uses the first glass powder #1, Example 2 uses the second glass powder #2, and Examples 3 and 4 use a mixture of the first glass powder and the second glass powder. Examples 1 to 3 are high silver content (silver content greater than 60%) terminal electrode silver paste formulas, and Example 4 is a low silver content (silver content of 47.7%) terminal electrode silver paste formula. The silver content determines the thickness of the rear electrode silver layer after sintering. Comparative Example 1 uses #3 granular glass powder.

[0034] Table 2. Examples and comparative examples formulations

[0035]

[0036] Note: (1) The proportions used in Table 2 are weight percentages; (2) Dow DC57 is an auxiliary leveling agent.

[0037] The terminal electrode silver paste is prepared by mixing, stirring and grinding according to the formula ratio in Table 2. The specific preparation method is as follows:

[0038] Step 1: Mix the resin ethyl cellulose and the diluent diethylene glycol butyl ether acetate (BCA) according to the proportions in Table 2, heat and dissolve, and cool to room temperature after the resin ethyl cellulose is completely dissolved; add the leveling agent Dow DC57 according to the proportions in Table 2, and stir evenly to obtain an organic carrier;

[0039] Step 2: Add different glass powders according to Table 2 into the organic carrier, stir evenly, and prepare glass slurry;

[0040] Step 3: Add different silver powders to the glass paste according to Table 2, stir evenly, and then pass the paste through a three-roll mill to obtain the terminal electrode silver paste; centrifuge the obtained terminal electrode silver paste for degassing and seal.

[0041] According to the above-mentioned raw materials and slurry preparation process, 5 different terminal electrode silver pastes were prepared in Examples 1 to 4 and Comparative Example 1, and used to prepare chip inductors for printing tests. Specifically, the terminal electrode silver paste is dip-coated on the ferrite core electrode (chip inductor model 3416, Zhejiang Zhonghan Electronic Technology Co., Ltd.) through a terminal sealing machine, and the subsequent baking conditions are 120°C / 15 minutes, and the sintering conditions are 665°C / 20 minutes. Afterwards, the 3416 chip inductor terminated with silver paste is electroplated with a nickel layer and a tin layer, thereby forming a ferrite core / end silver layer / nickel layer / tin layer structure from the inside to the outside on the electrode side to obtain a chip inductor.

[0042] The following tests are mainly performed on the terminated chip inductors:

[0043] 1. Scanning electron microscope (SEM) was used to observe the morphology after sintering;

[0044] 2. The thrust meter tests the welding adhesion of the inductor terminal electrodes. The specific steps are as follows: 1) Solder the electroplated chip inductor (the terminal electrodes of the chip inductor are ferrite core electrode, terminal silver layer, nickel layer and tin layer from the inside to the outside) to the copper plate using solder paste; 2) Fix the copper plate and use the thrust meter to push the inductor at a constant speed until it falls off and record the thrust peak.

[0045] The terminal electrode silver pastes of Examples 1-4 and Comparative Example 1 were respectively dip-coated onto the terminal electrodes of the 3416 chip inductor, dried at 120° C. for 15 minutes, and sintered at 665° C. for 20 minutes. Figure 2 The scanning electron microscope (SEM) images of the sintered rear end silver electrode, where (a) to (d) in Figure 2 correspond to Examples 1 to 4, and (e) corresponds to Example 1. By comparing the observations, it can be found that Figure 2 In (a) to (d), after high-temperature sintering, the end silver layer (the brighter part in the SEM image) forms a raised and continuous chain structure. These continuous silver raised structures can serve as anchor points for the subsequent electroplating growth of nickel and tin layers, and play a vital role in the thickness and electroplating speed of the subsequent electroplating layers. Figure 2 (d) is a low-silver-containing terminal electrode silver paste, so its surface silver protrusion density is lower than that of Examples 1 to 3. The adhesion of the glass body to the terminal silver layer plays a vital role. Figure 2 The glass body (the darker part in the SEM image) in (a) to (d) sinks after sintering to form a matrix structure: on the one hand, the glass body is tightly attached to the surface of the ferrite, and on the other hand, the glass body wraps the end silver electrode and embeds it in it, so that the glass body firmly connects and attaches the end silver layer (and subsequent nickel layer / tin layer) to the ferrite core electrode.

[0046] pass Figure 2 The SEM images shown show that the terminal electrode silver pastes prepared using flaky glass powder in Examples 1 to 4 all present a structure in which the silver layer is raised and the glass body is sunken. This structure is conducive to the formation of dense nickel and tin electroplating layers in subsequent processes. Figure 2 (e) is a SEM image of a silver-terminated electrode made of the commonly used granular glass powder used in Comparative Example 1. Figure 2 (a)~(d), Figure 2 (e) There are obvious differences, mainly in that the silver protrusions and glass body sinking are not obvious, and the area of ​​silver exposed on the glass body surface accounts for a small proportion. This makes the subsequent electroplating speed of the silver electrode at the middle end of comparative example 1 slower and the uniformity worse, and ultimately reduces the adhesion. The above results show that the flake glass powder has an important influence on reducing the melting point of the glass powder and the sinking of the glass body.

[0047] After the chip inductor is electroplated, a ferrite / terminal silver layer (containing glass) / nickel layer / tin layer structure is formed on the end electrode side from the inside to the outside. The chip inductors prepared in Examples 1 to 4 and Comparative Example 1 are soldered to a copper plate and the adhesion is tested (thrust peak value, 48 sets of thrust data are included in each example or comparative example). The test results show that the average thrust peak values ​​of the chip inductors corresponding to Examples 1 to 4 are 26.50N, 25.99N, 26.87N and 21.97N, respectively, while the average thrust peak value of Comparative Example 1 is 22.37N. Thrust tests were performed on Examples 1 to 4 and the comparative example. The results show that the thrust peak values ​​of Examples 1 to 3 are generally higher than the thrust values ​​of the comparative example, while the thrust value of Example 4 (low silver content formula) is equivalent to the thrust value of the comparative example. This shows that when the proportion of glass powder is equivalent, the flaky glass powder helps to improve the adhesion of the end electrode, which is consistent with the Figure 2 The silver protrusions formed in the SEM are closely related.

[0048] In summary, the flake glass powder plays a positive role in the sintering process of the terminal silver layer: (1) promoting the formation of silver protrusions, (2) promoting the sinking of the glass body after sintering, etc. The use of flake glass powder in the terminal electrode silver paste plays an important role in the preparation of high adhesion and high reliability chip inductors.

[0049] The embodiments described above are merely descriptions of preferred implementations of the present invention and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope of the present invention.

Claims

1. A silver paste for terminal electrodes of a chip inductor, characterized in that: The terminal electrode silver paste comprises silver powder, flaky glass powder, and an organic carrier; the particle size D of the flaky glass powder is 50 It is 0.5 to 10 μm, and the diameter / thickness ratio is 2 to 20.

2. The terminal electrode silver paste according to claim 1, characterized in that: The flaky glass powder comprises a first flaky glass powder and a second flaky glass powder; the particle size D of the first flaky glass powder is 50 The particle size D of the second flake glass powder is 1 to 5 μm; 50 is 0.5~2.5μm; the mass ratio of the first flaky glass powder to the second flaky glass powder is (0.8~1.2):

1.

3. The terminal electrode silver paste according to claim 1, characterized in that: The components of the flaky glass powder include SiO2, B2O3 and Al2O3.

4. The terminal electrode silver paste according to claim 1, characterized in that: The silver powder includes a first silver powder and a second silver powder; the particle size D of the first silver powder is 50 The particle size D of the second silver powder is 1 to 3 μm; 50 is 0.2-1 μm; the mass ratio of the first silver powder to the second silver powder is (8-20):

1.

5. The terminal electrode silver paste according to claim 1, characterized in that: The organic carrier comprises resin, diluent and auxiliary agent.

6. The terminal electrode silver paste according to claim 5, characterized in that: The resin is selected from at least one of ethyl cellulose, cellulose acetate butyrate, and polyvinyl butyral.

7. The terminal electrode silver paste according to claim 5, characterized in that: The diluent is selected from at least one of diethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, dibasic acid ester and terpineol.

8. The terminal electrode silver paste according to any one of claims 1 to 7, characterized in that: The terminal electrode silver paste comprises 40-80wt% of silver powder, 2-20wt% of flaky glass powder, 2-20wt% of resin, 10-50wt% of diluent, and 0.1-3wt% of auxiliary agent.

9. A chip inductor, characterized in that: The chip inductor is prepared using the terminal electrode silver paste as described in any one of claims 1 to 7.