Palladium-silver-copper terminal electrode slurry and preparation method and application thereof

Through the use of palladium-silver-copper end electrode paste, combined with silver powder, palladium powder and copper powder and glass powder containing SrO, BaO, and Li2O, the oxidation and mounting stability of MLCC products under humid and heat conditions are solved, and the problem of oxidation and installation stability of MLCC products is achieved. The improvement of high adhesion and sintering performance improves the service life and welding performance of the product.

CN118969354APending Publication Date: 2024-11-15GUANGDONG FENGHUA ADVANCED TECHNOLOGY (HOLDING) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411316916.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing MLCC products are prone to oxidation under humid and heat conditions. The welding layer is affected by ambient temperature or humidity, resulting in a reduction in mounting stability. The existing mounting process requires high and low temperature thermal shock experiments, which generates stress and causes cracking of ceramic media or welding layer. Impacts the service life of the product.

Method used

Palladium, silver and copper end electrode paste is made of 69% to 83% metal powder, 4% to 11% glass powder and 13% to 20% organic binder. Silver powder, palladium powder and copper powder are used to form metal powder. Combined with glass powder containing SrO, BaO, Li2O, and using an organic binder of acrylic resin and ethyl cellulose, grind to a fineness of ≤10μm to form a palladium silver copper end electrode paste, enhancing adhesion and binding force, and reducing sintering stress.

Benefits of technology

Improve the adhesion and bonding force between the palladium-silver-copper end electrode paste and the copper end electrode, reduce the sintering stress during the sintering process, reduce product cracking, improve welding performance and conductivity, and give MLCC products good mounting Stability and excellent conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969354A_ABST
    Figure CN118969354A_ABST
Patent Text Reader

Abstract

The invention relates to palladium-silver-copper terminal electrode slurry and a preparation method and application thereof, and belongs to the technical field of conductive materials containing metal or alloy. The palladium-silver-copper terminal electrode slurry comprises the following components in percentage by mass: 69%-83% of metal powder, 4%-11% of glass powder and 13%-20% of an organic adhesive, the metal powder is mainly composed of silver powder, palladium powder and copper powder, and the glass powder comprises SrO, BaO, Li2O and Na2O; the organic adhesive is mainly composed of a high polymer material, an organic solvent and an auxiliary agent, the high polymer material is at least one of acrylic resin, ethyl cellulose and hydroxyethyl cellulose, and the auxiliary agent is at least one of a dispersing agent, a flatting agent and a plasticizer. The copper end electrode of the chip multilayer ceramic capacitor coated with the palladium-silver-copper end electrode slurry has good welding performance and excellent conductivity after being sintered.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of conductive materials containing metals or alloys, and in particular to a palladium-silver-copper terminal electrode slurry and a preparation method and application thereof. Background Art

[0002] Chip multilayer ceramic capacitors (MLCC) are structures formed by stacking ceramic dielectric diaphragms with printed electrodes in an offset manner and sintering them at high temperature once to form ceramic chips, and then sealing metal layers (external electrodes) at both ends of the chip. It is currently one of the most widely used and fastest-growing electronic components. Most of the external electrodes use copper metal electrodes or silver metal electrodes, but because silver metal electrodes have high production costs and are prone to silver migration under hot and humid conditions, which affects the service life of the device, people began to use copper paste instead of silver paste to sinter and prepare copper metal electrodes, and nickel was plated on the surface of the copper metal electrode to form a barrier layer, and then tin or tin-lead was plated on the surface of the barrier layer to form a soldering layer. However, in actual application, it was found that the above-mentioned MLCC products are prone to oxidation of the soldering layer due to ambient temperature or humidity during placement, which affects their soldering performance. Moreover, the mounting process of existing MLCC products requires repeated high and low temperature thermal shock reliability tests under -55℃ to 150℃. The stress generated in this process can easily cause cracking of the ceramic dielectric or soldering layer, affecting the mounting stability of MLCC products. Using flexible conductive adhesive instead of tin for welding (bonding) can effectively alleviate the influence of stress generated during the mounting process to improve mounting stability. Therefore, there is an urgent need for a copper terminal electrode coating that can be directly welded with conductive adhesive without electroplating to improve the mounting stability of MLCC products. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a palladium-silver-copper terminal electrode slurry and a preparation method and application thereof.

[0004] To achieve the above object, the technical solution adopted by the present invention is:

[0005] In a first aspect, the present invention provides a palladium-silver-copper terminal electrode slurry, which comprises the following components by mass percentage:

[0006] 69% to 83% metal powder, 4% to 11% glass powder, 13% to 20% organic binder;

[0007] The metal powder is mainly composed of silver powder, palladium powder and copper powder;

[0008] The glass powder contains SrO, BaO, Li 2 O and Na 2 O;

[0009] The organic adhesive is mainly composed of polymer materials, organic solvents and additives; the polymer material is at least one of acrylic resin, ethyl cellulose and hydroxyethyl cellulose; the additive is at least one of dispersants, leveling agents and plasticizers.

[0010] The present invention uses silver powder, palladium powder and copper powder to form a metal powder, and mixes with SrO, BaO, Li 2 O and Na 2 The combination of the palladium-silver-copper terminal electrode slurry and the organic adhesive containing acrylic resin and / or ethyl cellulose can not only maintain a good impregnation effect when the palladium-silver-copper terminal electrode slurry is used to coat the copper terminal electrode of the chip-type multilayer ceramic capacitor, but also enhance the adhesion between the slurry layer (obtained by drying the palladium-silver-copper terminal electrode slurry) and the copper terminal electrode to prevent it from falling off during the sintering process. At the same time, it can also effectively reduce the sintering stress during the sintering process to reduce product cracking, and enhance the bonding force between the coating layer (obtained by sintering the slurry layer) and the copper terminal electrode, so that it has good welding performance and excellent conductive performance, thereby giving the chip-type multilayer ceramic capacitor product good mounting stability.

[0011] Optionally, the mass percentage of the metal powder in the palladium silver copper terminal electrode slurry can be 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, the mass percentage of the glass powder can be 5%, 6%, 7%, 8%, 9%, 10%, and the mass percentage of the organic binder can be 14%, 15%, 16%, 17%, 18%, 19%. In addition, the acrylic resin in the above-mentioned high-resolution material is preferably polyacrylic acid resin.

[0012] Preferably, the polymer material is a mixture of acrylic resin and ethyl cellulose. Optionally, the mass ratio of the acrylic resin to the ethyl cellulose is (8-15):(0.5-1.5); in terms of weight, the acrylic resin can be 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, and the ethyl cellulose can be 0.6 parts, 0.8 parts, 1 part, 1.2 parts, 1.4 parts.

[0013] The combination of acrylic resin and ethyl cellulose can not only make the polymer material decompose and discharge more fully during the sintering process, thereby reducing the carbon residue in the palladium silver copper terminal electrode slurry to improve its sintering and density; it can also make the polymer material have good toughness and adhesion to the copper terminal electrode, thereby making the palladium silver copper terminal electrode slurry have a good impregnation appearance and excellent impact resistance.

[0014] Optionally, the dispersant may be at least one of aliphatic amide and paraffin, the leveling agent may be at least one of acrylic acid and silicone, and the plasticizer may be at least one of citrate and polyester.

[0015] As a preferred embodiment of the palladium-silver-copper terminal electrode slurry of the present invention, the mass ratio of silver powder, palladium powder and copper powder in the metal powder is (60-70):(2-7):(2-7). Studies have found that the metal powder composed of silver powder, palladium powder and copper powder in the above mass ratio can make the electrode slurry sintered film layer have better density, weldability and conductivity.

[0016] Optionally, in parts by weight, the silver powder in the above-mentioned metal powder can be 61 parts, 62 parts, 63 parts, 64 parts, 65 parts, 66 parts, 67 parts, 68 parts, and 69 parts; the palladium powder can be 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts, 6 parts, and 6.5 parts; and the copper powder can be 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts, 6 parts, and 6.5 parts.

[0017] As a preferred embodiment of the palladium silver copper terminal electrode paste of the present invention, based on the total mass of the glass powder, the SrO in the glass powder is 14wt% to 21wt%, the BaO is 2wt% to 7wt%, and the Li 2 O is 0.4wt% to 2wt%, Na 2 O is 0.02wt% to 0.2wt%.

[0018] Optionally, the mass percentage of SrO in the glass powder may be 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%; the mass percentage of BaO may be 3wt%, 4wt%, 5wt%, 6wt%; the mass percentage of Li 2 The mass percentage of O can be specifically 0.5wt%, 0.8wt%, 1wt%, 1.3wt%, 1.5wt%, 1.8wt%; Na 2 The mass percentage of O can specifically be 0.05wt%, 0.08wt%, 0.1wt%, 0.12wt%, 0.15wt%, or 0.17wt%.

[0019] The study found that the above content range of SrO, BaO, Li 2 O、Na 2 O work together to better reduce the softening temperature of the glass powder, thereby more effectively reducing the sintering stress of the palladium-silver-copper terminal electrode slurry during the sintering process, thereby avoiding cracking; moreover, it also helps to improve the toughness of the glass system to enhance the sintering strength of the product.

[0020] As a preferred embodiment of the palladium silver copper terminal electrode paste of the present invention, the glass powder further comprises ZnO, SiO 2 , CuO, B 2 O 3 、CaO、Al 2 O 3 .

[0021] As a preferred embodiment of the palladium silver copper terminal electrode paste of the present invention, based on the total mass of the glass powder, the ZnO in the glass powder is 28wt% to 35wt%, the SiO 2 20wt%~27wt%, CuO 13wt%~20wt%, B 2 O 3 2wt%~7wt%, CaO 0.5wt%~3wt%, Al 2 O 3 It is 0.5wt%~3wt%.

[0022] Optionally, the mass percentage of ZnO in the glass powder may be 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, or 34wt%; 2 The mass percentage of B can be 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%; the mass percentage of CuO can be 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%; 2 O 3 The mass percentage of can be 3wt%, 4wt%, 5wt%, 6wt%; the mass percentage of CaO can be 1wt%, 1.5wt%, 2wt%, 2.5wt%; Al 2 O 3 The mass percentage may specifically be 1wt%, 1.5wt%, 2wt%, or 2.5wt%.

[0023] As a preferred embodiment of the palladium-silver-copper terminal electrode paste of the present invention, the silver powder is at least one of spherical silver powder and flaky silver powder; the particle size D50 of the spherical silver powder is 0.3-2 μm, and the particle size D50 of the flaky silver powder is 5-10 μm. Optionally, the particle size D50 of the spherical silver powder can be 0.4 μm, 0.6 μm, 0.8 μm, 1 μm, 1.2 μm, 1.4 μm, 1.6 μm, 1.8 μm, and the particle size D50 of the flaky silver powder can be 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm.

[0024] As a preferred embodiment of the palladium-silver-copper terminal electrode slurry of the present invention, the particle size D50 of the palladium powder is 0.3-2 μm. Optionally, the particle size D50 of the palladium powder can be 0.4 μm, 0.6 μm, 0.8 μm, 1 μm, 1.2 μm, 1.4 μm, 1.6 μm, 1.8 μm.

[0025] As a preferred embodiment of the palladium-silver-copper terminal electrode slurry of the present invention, the particle size D50 of the copper powder is 1.5-5.5 μm. Optionally, the particle size D50 of the copper powder can be 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, or 5 μm.

[0026] The particle size D50 of the silver powder, palladium powder and copper powder can be measured by a laser particle size analyzer.

[0027] The metal powder composed of silver powder, palladium powder and copper powder in the above-mentioned particle size range can enable the palladium-silver-copper terminal electrode slurry to be sintered at a lower temperature to reduce sintering stress and thus reduce product cracking; at the same time, it can also better inhibit the metal powder from prematurely densifying during the sintering process, which may cause the sintered glass to float and the appearance of bubbles, thereby maintaining the product with excellent electrical properties and weldability; it can also enable the palladium-silver layer to have better crystal density, thereby better interacting with the copper powder to enhance the bonding performance with the copper terminal electrode.

[0028] As a preferred embodiment of the palladium silver copper terminal electrode slurry of the present invention, the mass ratio of the polymer material, the organic solvent and the auxiliary agent is (15-45): (50-80): (1-10). Optionally, by weight, the polymer material can be 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, the organic solvent can be 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, and the auxiliary agent can be 2 parts, 4 parts, 6 parts, 8 parts. Studies have found that when the mass ratio between the polymer material, the organic solvent and the auxiliary agent is within the above range, it can not only make the electrode slurry have a more suitable viscosity and a higher drying film strength, but also help to improve the appearance performance of the product.

[0029] In a second aspect, the present invention provides a method for preparing the above-mentioned palladium silver copper terminal electrode slurry, which comprises the following steps: mixing metal powder, glass powder and organic binder evenly, and grinding the mixture to a fineness of ≤10 μm to obtain palladium silver copper terminal electrode slurry.

[0030] In the above preparation method, silver powder, palladium powder and copper powder can be mixed first, and then mixed with glass powder and organic binder, or silver powder, palladium powder and copper powder can be directly mixed with glass powder and organic binder. The grinding temperature is 16-40°C, and the grinding fineness is controlled to be ≤10μm to promote more uniform dispersion of components in the electrode slurry to maintain the consistency of the electrode slurry components; at the same time, it can also effectively avoid appearance problems such as electrode nodules caused by excessive product fineness.

[0031] The organic binder can be obtained by adding the polymer material and the auxiliary agent to an organic solvent at 75 to 90° C. and stirring and dissolving for 2 to 4 hours. The organic solvent can be an alcohol (specifically, it can be at least one of terpineol, butyl carbitol, and 2-ethylhexanol) and / or a lipid (specifically, it can be at least one of diethylene glycol ethyl ether acetate and diethylene glycol butyl ether acetate).

[0032] The glass powder can be prepared by mixing various glass components (ZnO, SiO 2 , CuO, B 2 O 3 、CaO、Al 2 O 3 、SrO、BaO、Li 2 O、Na 2 O) After being uniformly mixed, the mixture is melted at 1200-1400° C., quenched, crushed, and sieved to obtain a powder with a particle size D50 of 2-6 μm. Glass powder within this particle size range is more conducive to regulating the sintering temperature of the palladium-silver-copper terminal electrode slurry.

[0033] In a third aspect, the present invention provides a use of the above-mentioned palladium-silver-copper terminal electrode slurry in the preparation of a chip-type multilayer ceramic capacitor.

[0034] In a fourth aspect, the present invention provides a chip-type multilayer ceramic capacitor, which includes a ceramic dielectric, an inner electrode and an outer terminal electrode; the outer terminal electrode is a copper metal electrode, and a coating layer is provided on the surface of the copper metal electrode; the coating layer is prepared using the above-mentioned palladium silver copper terminal electrode slurry.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] The present invention uses silver powder, palladium powder and copper powder to form a metal powder, and mixes with SrO, BaO, Li 2 O and Na 2The combination of palladium-silver-copper terminal electrode slurry and an organic adhesive containing acrylic resin and / or ethyl cellulose can not only maintain a good impregnation effect when the palladium-silver-copper terminal electrode slurry is used to coat the copper terminal electrode of the chip-type multilayer ceramic capacitor, but also enhance the adhesion between the slurry layer and the copper terminal electrode to prevent it from falling off during the sintering process. At the same time, it can also effectively reduce the sintering stress during the sintering process to reduce product cracking, and improve the bonding force between the coating layer and the copper terminal electrode, so that it has good welding performance and excellent conductive performance, thereby giving the chip-type multilayer ceramic capacitor product good mounting stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a schematic diagram of the product structure of the palladium-silver-copper terminal electrode slurry coated with the MLCC copper terminal electrode before sintering;

[0038] Figure 2 The surface SEM image (A, magnification of 3000 times) and cross-sectional laser microscope image (B, magnification of 20 times) of the MLCC copper terminal electrode coated with the palladium-silver-copper terminal electrode slurry after sintering in Example 1;

[0039] Figure 3 The surface SEM image (A, magnification of 3000 times) and cross-sectional laser microscope image (B, magnification of 20 times) of the MLCC copper terminal electrode coated with the palladium-silver-copper terminal electrode slurry after sintering in Example 2;

[0040] Figure 4 The surface SEM image (A, magnification of 3000 times) and cross-sectional laser microscope image (B, magnification of 20 times) of the MLCC copper terminal electrode coated with the palladium-silver-copper terminal electrode slurry after sintering in Example 3;

[0041] Figure 5 The surface SEM image (A, magnification of 3000 times) and cross-sectional laser microscope image (B, magnification of 20 times) of the MLCC copper terminal electrode coated with the palladium-silver-copper terminal electrode slurry after sintering in Example 4;

[0042] Figure 6 The surface SEM image (A, magnification of 3000 times) and cross-sectional laser microscope image (B, magnification of 20 times) of the MLCC copper terminal electrode coated with the palladium-silver-copper terminal electrode slurry after sintering in Example 5;

[0043] Figure 7 The surface SEM image (A, magnification of 3000 times) and cross-sectional laser microscope image (B, magnification of 20 times) of the MLCC copper terminal electrode coated with the palladium-silver-copper terminal electrode slurry after sintering in Example 6;

[0044] Figure 8The surface SEM image (A, magnification of 3000 times) and cross-sectional laser microscope image (B, magnification of 20 times) of the MLCC copper terminal electrode coated with the palladium-silver-copper terminal electrode slurry after sintering in Example 7;

[0045] Fig. 9 The surface SEM image (A, magnification of 3000 times) and cross-sectional laser microscope image (B, magnification of 20 times) of the MLCC copper terminal electrode coated with palladium silver copper terminal electrode slurry after sintering in Comparative Example 1;

[0046] Fig.10 The surface SEM image (A, magnification of 3000 times) and cross-sectional laser microscope image (B, magnification of 20 times) of the MLCC copper terminal electrode coated with palladium-silver-copper terminal electrode slurry after sintering in Comparative Example 2;

[0047] Fig.11 The surface SEM image (A, magnification of 3000 times) and cross-sectional laser microscope image (B, magnification of 20 times) of the MLCC copper terminal electrode coated with palladium-silver-copper terminal electrode slurry after sintering in Comparative Example 3;

[0048] Fig.12 These are the surface SEM image (A, magnification of 3000 times) and the cross-sectional laser microscope image (B, magnification of 20 times) of the MLCC copper terminal electrode coated with the palladium-silver-copper terminal electrode slurry after sintering in Comparative Example 4. DETAILED DESCRIPTION

[0049] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0050] Unless otherwise specified, other materials, reagents, etc. used in the examples can be obtained from commercial sources.

[0051] Example 1

[0052] An embodiment of the palladium-silver-copper terminal electrode slurry of the present invention, the components and weight fractions of the palladium-silver-copper terminal electrode slurry described in this embodiment are as follows:

[0053] Component a-metal powder (74%), by weight, includes the following components:

[0054] 25 parts of spherical silver powder, 35 parts of flake silver powder, 7 parts of palladium powder, 7 parts of copper powder;

[0055] Component b-glass powder (9%), by weight percentage, consists of the following components:

[0056] 2.7% ZnO, 2.07% SiO 2 , 1.44% CuO, 0.36% B 2 O3 , 0.18% CaO, 0.13% Al 2 O 3 , 1.53% SrO, 0.45% BaO, 0.13% Li 2 O, 0.01% Na 2 O;

[0057] Component c-organic binder (17%), by weight, includes the following components:

[0058] The polymer material (6 parts) consists of 5.5 parts of polyacrylic acid resin and 0.5 parts of ethyl cellulose;

[0059] The organic solvent (10 parts) consists of 1 part of butyl carbitol, 1 part of 2-ethylhexanol, 2 parts of diethylene glycol ethyl ether acetate and 6 parts of diethylene glycol butyl ether acetate;

[0060] The additive (1 part) is composed of 0.5 parts of dispersant (oleic acid amide) and 0.5 parts of leveling agent (polyether siloxane).

[0061] The preparation method of the palladium-silver-copper terminal electrode slurry described in this embodiment is: metal powder, glass powder and organic binder are evenly mixed, and ground until the fineness of the mixture is ≤10 μm to obtain the palladium-silver-copper terminal electrode slurry.

[0062] Example 2

[0063] An embodiment of the palladium-silver-copper terminal electrode slurry of the present invention, the components and weight fractions of the palladium-silver-copper terminal electrode slurry described in this embodiment are as follows:

[0064] Component a-metal powder (72%), by weight, includes the following components:

[0065] 29 parts of spherical silver powder, 32 parts of flake silver powder, 7 parts of palladium powder, 4 parts of copper powder;

[0066] Component b-glass powder (11%), by weight percentage, consists of the following components:

[0067] 3.74% ZnO, 2.31% SiO 2 , 1.98% CuO, 0.66% B 2 O 3 , 0.11% CaO, 0.11% Al 2 O 3 , 1.65% SrO, 0.33% BaO, 0.1% Li 2 O, 0.01% Na 2 O;

[0068] Component c-organic binder (17%), by weight, includes the following components:

[0069] The polymer material (6 parts) consists of 5.5 parts of polyacrylic acid resin and 0.5 parts of ethyl cellulose;

[0070] The organic solvent (10 parts) consists of 1 part of butyl carbitol, 1 part of 2-ethylhexanol, 2 parts of diethylene glycol ethyl ether acetate and 6 parts of diethylene glycol butyl ether acetate;

[0071] The additive (1 part) is composed of 0.5 parts of dispersant (oleic acid amide) and 0.5 parts of leveling agent (polyether siloxane).

[0072] The preparation method of the palladium silver copper terminal electrode slurry described in this embodiment is the same as that in Example 1.

[0073] Example 3

[0074] An embodiment of the palladium-silver-copper terminal electrode slurry of the present invention, the components and mass fractions of the palladium-silver-copper terminal electrode slurry described in this embodiment are as follows:

[0075] Component a-metal powder (74%), by weight, includes the following components:

[0076] 30 parts of spherical silver powder, 32 parts of flake silver powder, 6 parts of palladium powder, 6 parts of copper powder;

[0077] Component b-glass powder (8%), by weight percentage, consists of the following components:

[0078] 2.64% ZnO, 1.76% SiO 2 , 1.36% CuO, 0.4% B 2 O 3 , 0.08% CaO, 0.08% Al 2 O 3 , 1.28% SrO, 0.4% BaO, 0.14% Li 2 O, 0.02% Na 2 O;

[0079] Component c-organic binder (18%), by weight, includes the following components:

[0080] The polymer material (6 parts) consists of 5.5 parts of polyacrylic acid resin and 0.5 parts of ethyl cellulose;

[0081] The organic solvent (11 parts) consists of 1 part of butyl carbitol, 1 part of 2-ethylhexanol, 2.5 parts of diethylene glycol ethyl ether acetate and 6.5 parts of diethylene glycol butyl ether acetate;

[0082] The additive (1 part) is composed of 0.5 parts of dispersant (oleic acid amide) and 0.5 parts of leveling agent (polyether siloxane).

[0083] The preparation method of the palladium silver copper terminal electrode slurry described in this embodiment is the same as that in Example 1.

[0084] Example 4

[0085] An embodiment of the palladium-silver-copper terminal electrode slurry of the present invention, the components and mass fractions of the palladium-silver-copper terminal electrode slurry described in this embodiment are as follows:

[0086] Component a-metal powder (74%), by weight, includes the following components:

[0087] 33 parts of spherical silver powder, 30 parts of flake silver powder, 5 parts of palladium powder, 6 parts of copper powder;

[0088] Component b-glass powder (8%), by weight percentage, consists of the following components:

[0089] 2.48% ZnO, 1.76% SiO 2 , 1.52% CuO, 0.32% B 2 O 3 , 0.16% CaO, 0.12% Al 2 O 3 , 1.20% SrO, 0.32% BaO, 0.11% Li 2 O, 0.01% Na 2 O;

[0090] Component c-organic binder (18%), by weight, includes the following components:

[0091] The polymer material (6 parts) is polyacrylic acid resin;

[0092] The organic solvent (11 parts) consists of 1 part of butyl carbitol, 1 part of 2-ethylhexanol, 2.5 parts of diethylene glycol ethyl ether acetate and 6.5 parts of diethylene glycol butyl ether acetate;

[0093] The additive (1 part) is composed of 0.5 parts of dispersant (oleic acid amide) and 0.5 parts of leveling agent (polyether siloxane).

[0094] The preparation method of the palladium silver copper terminal electrode slurry described in this embodiment is the same as that in Example 1.

[0095] Example 5

[0096] An embodiment of the palladium-silver-copper terminal electrode slurry of the present invention, the components and mass fractions of the palladium-silver-copper terminal electrode slurry described in this embodiment are as follows:

[0097] Component a-metal powder (74%), by weight, includes the following components:

[0098] 35 parts of spherical silver powder, 30 parts of flake silver powder, 4 parts of palladium powder, 5 parts of copper powder;

[0099] Component b-glass powder (7%), by weight percentage, consists of the following components:

[0100] 2.03% ZnO, 1.82% SiO 2 , 1.12% CuO, 0.35% B 2 O 3 , 0.07% CaO, 0.07% Al 2 O 3 , 1.26% SrO, 0.21% BaO, 0.06% Li 2 O, 0.01% Na 2 O;

[0101] Component c-organic binder (19%), by weight, includes the following components:

[0102] The polymer material (6 parts) is polyacrylic acid resin;

[0103] The organic solvent (12 parts) consists of 0.5 parts of terpineol, 1.5 parts of butyl carbitol, 1 part of 2-ethylhexanol, 2.5 parts of diethylene glycol ethyl ether acetate and 6.5 parts of diethylene glycol butyl ether acetate;

[0104] The additive (1 part) is composed of 0.5 parts of dispersant (oleic acid amide) and 0.5 parts of leveling agent (polyether siloxane).

[0105] The preparation method of the palladium silver copper terminal electrode slurry described in this embodiment is the same as that in Example 1.

[0106] Example 6

[0107] An embodiment of the palladium-silver-copper terminal electrode slurry of the present invention, the components and mass fractions of the palladium-silver-copper terminal electrode slurry described in this embodiment are as follows:

[0108] Component a-metal powder (74%), by weight, includes the following components:

[0109] 40 parts of spherical silver powder, 29 parts of flake silver powder, 3 parts of palladium powder, 2 parts of copper powder;

[0110] Component b-glass powder (7%), by weight percentage, consists of the following components:

[0111] 2.03% ZnO, 1.61% SiO 2 , 1.33% CuO, 0.42% B2 O 3 , 0.17% CaO, 0.14% Al 2 O 3 , 1.05% SrO, 2.00% BaO, 0.04% Li 2 O, 0.01% Na 2 O;

[0112] Component c-organic binder (19%), by weight, includes the following components:

[0113] The polymer material (6 parts) is polyacrylic acid resin;

[0114] The organic solvent (12 parts) consists of 0.5 parts of terpineol, 1.5 parts of butyl carbitol, 1 part of 2-ethylhexanol, 2.5 parts of diethylene glycol ethyl ether acetate and 6.5 parts of diethylene glycol butyl ether acetate;

[0115] The additive (1 part) is composed of 0.5 parts of dispersant (oleic acid amide) and 0.5 parts of leveling agent (polyether siloxane).

[0116] The preparation method of the palladium silver copper terminal electrode slurry described in this embodiment is the same as that in Example 1.

[0117] Example 7

[0118] An embodiment of the palladium-silver-copper terminal electrode slurry of the present invention, the components and mass fractions of the palladium-silver-copper terminal electrode slurry described in this embodiment are as follows:

[0119] Component a-metal powder (76%), by weight, includes the following components:

[0120] 45 parts of spherical silver powder, 25 parts of flake silver powder, 2 parts of palladium powder, 4 parts of copper powder;

[0121] Component b-glass powder (5%), by weight percentage, consists of the following components:

[0122] 1.45% ZnO, 1.10% SiO 2 , 0.70% CuO, 0.15% B 2 O 3 , 0.12% CaO, 0.12% Al 2 O 3 , 1.00% SrO, 0.30% BaO, 0.05% Li 2 O, 0.01% Na 2 O;

[0123] Component c-organic binder (19%), by weight, includes the following components:

[0124] The polymer material (5 parts) is 4.7 parts of polyacrylic acid resin and 0.3 parts of ethyl cellulose;

[0125] The organic solvent (12.8 parts) is composed of 1 part of terpineol, 1 part of butyl carbitol, 2 parts of 2-ethylhexanol, 2 parts of diethylene glycol ethyl ether acetate and 6.8 parts of diethylene glycol butyl ether acetate;

[0126] The auxiliary agent (1.2 parts) is composed of 0.5 parts of a dispersant (oleic acid amide), 0.5 parts of a leveling agent (polyether siloxane) and 0.2 parts of a plasticizer (tributyl citrate).

[0127] The preparation method of the palladium silver copper terminal electrode slurry described in this embodiment is the same as that in Example 1.

[0128] Comparative Example 1

[0129] A comparative example of the palladium-silver-copper terminal electrode slurry of the present invention, the palladium-silver-copper terminal electrode slurry in this comparative example is basically the same as that in Example 1, except that:

[0130] Component a-metal powder (74%), including the following components by weight: 25 parts of spherical silver powder, 35 parts of flaky silver powder, and 14 parts of copper powder.

[0131] The preparation method of the palladium silver copper terminal electrode slurry described in this embodiment is the same as that in Example 1.

[0132] Comparative Example 2

[0133] A comparative example of the palladium-silver-copper terminal electrode slurry of the present invention, the palladium-silver-copper terminal electrode slurry in this comparative example is basically the same as that in Example 1, except that:

[0134] Component a-metal powder (74%), including the following components by weight: 25 parts of spherical silver powder, 35 parts of flaky silver powder, and 14 parts of palladium powder.

[0135] The preparation method of the palladium silver copper terminal electrode slurry described in this embodiment is the same as that in Example 1.

[0136] Comparative Example 3

[0137] A comparative example of the palladium-silver-copper terminal electrode slurry of the present invention, the palladium-silver-copper terminal electrode slurry in this comparative example is basically the same as that in Example 1, except that:

[0138] Component b-glass powder (0%);

[0139] Component c-organic binder (26%), by weight, includes the following components:

[0140] The polymer material (6 parts) consists of 5.5 parts of polyacrylic acid resin and 0.5 parts of ethyl cellulose;

[0141] The organic solvent (19 parts) consists of 1 part of butyl carbitol, 1 part of 2-ethylhexanol, 2 parts of diethylene glycol ethyl ether acetate and 15 parts of diethylene glycol butyl ether acetate;

[0142] The additive (1 part) is composed of 0.5 parts of dispersant (oleic acid amide) and 0.5 parts of leveling agent (polyether siloxane).

[0143] The preparation method of the palladium silver copper terminal electrode slurry described in this embodiment is the same as that in Example 1.

[0144] Comparative Example 4

[0145] A comparative example of the palladium-silver-copper terminal electrode slurry of the present invention, the palladium-silver-copper terminal electrode slurry in this comparative example is basically the same as that in Example 1, except that:

[0146] Component b-glass powder (9%), by weight percentage, includes the following components:

[0147] 3.42% ZnO, 2.52% SiO 2 , 1.89% CuO, 0.63% B 2 O 3 , 0.27% CaO, 0.27% Al 2 O 3 .

[0148] The preparation method of the palladium silver copper terminal electrode slurry described in this embodiment is the same as that in Example 1.

[0149] Performance Testing

[0150] The palladium-silver-copper terminal electrode pastes in Examples 1 to 7 and Comparative Examples 1 to 4 were respectively coated on the copper layer at both ends of the MLCC product, dried at 100 to 150°C, and then heated at 580 to 650°C, N 2 After sintering in atmosphere for 10 to 20 minutes, the Figure 1 The MLCC products shown were subjected to the following performance tests.

[0151] 1. Scanning electron microscope test

[0152] according to Figures 2 to 8 It can be seen that the surface crystal appearance of the MLCC copper terminal electrodes coated with the palladium-silver-copper terminal electrode slurry in Examples 1 to 7 after sintering is normal, and there is no glass floating phenomenon; at the same time, it can be seen from the corresponding cross-sectional diagram that the slurry is well bonded to the copper terminal electrode without any gaps, indicating that the palladium-silver-copper terminal electrode slurry of the present invention is coated on the MLCC copper terminal electrode, and the coating layer formed after sintering is tightly bonded to the copper terminal electrode, which is beneficial to promoting the improvement of the conductive performance.

[0153] according to Fig. 9 and 10It can be found that when a mixture of silver powder and copper powder is used as the metal powder and the corresponding palladium-silver-copper terminal electrode slurry is used to coat the MLCC copper terminal electrode for sintering, the glass powder floats up during the sintering process to form a diaphragm, resulting in poor contact between the coating layer and the substrate, thereby significantly increasing the contact resistance; and when a mixture of silver powder and palladium powder is used as the metal powder and the corresponding palladium-silver-copper terminal electrode slurry is used to coat the MLCC copper terminal electrode for sintering, the coating layer formed has poor density, loose interior, and poor component connection, which also leads to a significant increase in contact resistance.

[0154] according to Fig.11 and 12 It can be seen that when the MLCC copper terminal electrode is sintered by coating the palladium-silver-copper terminal electrode slurry without adding glass powder, the formed coating layer has poor bonding with the copper terminal electrode, resulting in obvious pores between the two, which significantly increases the contact resistance; while the MLCC copper terminal electrode slurry without adding SrO, BaO, and Li 2 O and Na 2 The MLCC copper terminal electrode is coated with palladium-silver-copper terminal electrode slurry of O glass powder and sintered. Although it can improve the bonding between the coating layer and the copper terminal electrode, it will cause the copper terminal electrode layer to fall off, making it difficult to effectively reduce the contact resistance.

[0155] 2. Contact resistance test

[0156] Test method: Directly test with LCR bridge tester after welding.

[0157] After testing, the contact resistance of the MLCC copper terminal electrodes coated with the palladium-silver-copper terminal electrode slurry in the above-mentioned Examples 1 to 7 after sintering were 1.7Ω, 1.9Ω, 0.7Ω, 1.0Ω, 1.5Ω, 1.3Ω, and 1.6Ω, respectively, while the contact resistance of the MLCC copper terminal electrodes coated with the palladium-silver-copper terminal electrode slurry in the above-mentioned Comparative Examples 1 to 4 after sintering were 65.2Ω, 47.1Ω, 868.5Ω, and 1326.8Ω, respectively, which indicates that the MLCC copper terminal electrodes coated with the palladium-silver-copper terminal electrode slurry of the present invention have good conductivity after sintering.

[0158] 3. Welding test

[0159] Test method: The products coated with the palladium-silver-copper terminal electrode slurry in Examples 1 to 7 are adhered to the substrate through the resin slurry and can be tightly fixed on the substrate after curing. This shows that the MLCC products coated with the copper terminal electrodes using the palladium-silver-copper terminal electrode slurry of the present invention and sintered have good weldability and can be directly used for circuit board welding without electroplating.

[0160] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A palladium-silver-copper terminal electrode slurry, characterized in that: Calculated by weight percentage, it includes the following components: 69% to 83% metal powder, 4% to 11% glass powder, 13% to 20% organic binder; The metal powder is mainly composed of silver powder, palladium powder and copper powder; The glass powder comprises SrO, BaO, Li2O and Na2O; The organic adhesive is mainly composed of polymer materials, organic solvents and additives; the polymer material is at least one of acrylic resin, ethyl cellulose and hydroxyethyl cellulose; the additive is at least one of dispersants, leveling agents and plasticizers.

2. The palladium-silver-copper terminal electrode slurry according to claim 1, characterized in that: The mass ratio of silver powder, palladium powder and copper powder in the metal powder is (60-70):(2-7):(2-7).

3. The palladium-silver-copper terminal electrode slurry according to claim 1, characterized in that: Based on the total mass of the glass powder, the glass powder contains 14wt% to 21wt% SrO, 2wt% to 7wt% BaO, 0.4wt% to 2wt% Li2O, and 0.02wt% to 0.2wt% Na2O.

4. The palladium-silver-copper terminal electrode slurry according to claim 1, characterized in that: The glass powder also contains ZnO, SiO2, CuO, B2O3, CaO, and Al2O3.

5. The palladium-silver-copper terminal electrode slurry according to claim 4, characterized in that: Based on the total mass of the glass powder, the ZnO in the glass powder is 28wt% to 35wt%, SiO2 is 20wt% to 27wt%, CuO is 13wt% to 20wt%, B2O3 is 2wt% to 7wt%, CaO is 0.5wt% to 3wt%, and Al2O3 is 0.5wt% to 3wt%.

6. The palladium-silver-copper terminal electrode slurry according to claim 1, characterized in that: At least one of the following (I) to (III): (I) the silver powder is at least one of spherical silver powder and flaky silver powder; the particle size D50 of the spherical silver powder is 0.3 to 2 μm, and the particle size D50 of the flaky silver powder is 5 to 10 μm; (II) the particle size D50 of the palladium powder is 0.3 to 2 μm; (III) The particle size D50 of the copper powder is 1.5 to 5.5 μm.

7. The palladium-silver-copper terminal electrode slurry according to claim 1, characterized in that: The mass ratio of the polymer material, the organic solvent and the auxiliary agent is (15-45):(50-80):(1-10).

8. The method for preparing the palladium-silver-copper terminal electrode slurry according to any one of claims 1 to 7, characterized in that: The following steps are involved: The metal powder, glass powder and organic binder are evenly mixed and ground to a mixture fineness of ≤10 μm to obtain palladium silver copper terminal electrode slurry.

9. Use of the palladium-silver-copper terminal electrode slurry according to any one of claims 1 to 7 in the preparation of chip-type multilayer ceramic capacitors.

10. A chip-type multilayer ceramic capacitor, comprising a ceramic dielectric, an inner electrode and an outer terminal electrode, characterized in that: The outer terminal electrode is a copper metal electrode, and a coating layer is provided on the surface of the copper metal electrode; the coating layer is prepared by using the palladium silver copper terminal electrode slurry described in any one of claims 1 to 7.