Low-temperature co-fired gold paste, preparation method and method for printing and sintering low-temperature co-fired gold paste on substrate
By adding glass powder and inorganic additives to the low-temperature co-burning gold paste, and using surface modifiers to form hexagonal and spherical gold powder, combined with gradient sintering technology, the existing gold paste is solved. The stress and conductivity of the existing gold paste during co-burning is insufficient. Problem, high performance and low cost low temperature co-burning slurry is achieved, suitable for a variety of electronic components.
Patent Information
- Application Number
- CN202411368759.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-15
AI Technical Summary
The existing low-temperature co-burning gold slurry does not match the thermal expansion coefficient of the ceramic substrate during co-burning, resulting in internal stress, affecting device reliability, and insufficient conductivity and sintering density, which makes the preparation cost high, limiting its in large-scale production. application.
Low-temperature co-burning gold paste of 73-80 wt% gold powder, 1-5 wt% glass powder, 1-5 wt% inorganic additives, and 10-25 wt% organic carriers are used to form a hexagonal and spherical gold powder coexisting through a surface modification agent, and combined with Gradient sintering technology optimizes the sintering process to reduce internal stress and improve conductivity.
It realizes good co-fired adaptability between gold paste and ceramic substrate, improves sintering performance and conductivity, reduces the internal stress and warping of the device, enhances the mechanical strength and dielectric properties of the substrate, and is suitable for LTCC inner layer, Surface layer and pore-filled slurry.
Smart Images

Figure CN118969355A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new information electronic materials, and in particular relates to a low temperature co-fired gold paste, a preparation method and a method for printing and sintering the paste on a substrate. Background Art
[0002] The development trend of microelectronic packaging includes high signal transmission speed, high wiring density, high reliability and low cost. Low Temperature Co-fired Ceramics (LTCC) can use a variety of highly conductive metals such as gold, silver, and copper to make high-density, high-precision metal layers, thereby achieving integration.
[0003] LTCC is a combination of powder preparation, slurry production, tape casting, molding and lamination. By using modified ceramics as thick film substrates, printing silver, gold or copper paste as internal electrodes, and then laminating and co-firing, various passive devices such as antennas, filters, baluns, couplers can be manufactured, or passive components can be packaged and integrated into three-dimensional substrates to achieve miniaturization and high performance of electronic devices.
[0004] In LTCC technology, gold paste, as a conductive material, is a key component for realizing circuit interconnection, and its performance directly affects the conductivity and reliability of LTCC devices. However, the gold paste used in the prior art has several limitations in the low-temperature co-firing process. First, the thermal expansion coefficients of the gold paste and the ceramic substrate do not match, resulting in internal stress during the co-firing process, which affects the reliability of the device. Secondly, the conductivity and sintering density of the existing gold paste cannot meet the growing high-performance requirements. In addition, the high preparation cost of gold paste limits its application in large-scale production.
[0005] The present invention provides a low-temperature co-fired gold paste with good co-fired adaptability, multi-purpose, good sintering performance and excellent conductivity, so as to achieve wider application in the electronics industry. Summary of the invention
[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides a low-temperature co-fired gold paste, a preparation method and a method for printing and sintering the paste on a substrate.
[0007] To achieve the above object, the technical solution adopted by the present invention is: a low temperature co-fired gold paste, comprising the following raw materials in percentage by weight: 73-80wt% gold powder, 1-5wt% glass powder, 1-5wt% inorganic additives, and 10-25wt% organic carrier;
[0008] The preparation method of the gold powder comprises the following steps: adding ammonia water to a chloroauric acid solution to adjust the pH to 7-8 to obtain a fulminate gold solution; adding concentrated hydrochloric acid to the fulminate gold solution to adjust the pH to 1-2, then adding a surface modifier and stirring, and then adding a reducing agent to react to obtain a reaction solution containing gold powder; and allowing the reaction solution to stand, separate, wash, and dry to obtain the gold powder;
[0009] The surface modifier is at least one of hexadecyltrimethylammonium bromide, 11-mercaptoundecanoic acid and polyacrylic acid.
[0010] As a preferred embodiment of the present invention, the gold powder is a mixture of hexagonal flakes and a small amount of spheres, with a purity of ≥99.95%, an average particle size of less than 10 μm, and a uniform particle size.
[0011] The present invention forms a hexagonal and spherical coexistence morphology by using at least one surface modifier selected from hexadecyltrimethylammonium bromide, 11-mercaptoundecanoic acid, and polyacrylic acid. The gold powder with the coexistence morphology of hexagonal and spherical shapes helps to reduce the viscosity of the slurry, improve fluidity, and improve the compactness of the film layer after sintering, the resolution and conductivity of the electrode.
[0012] As a preferred embodiment of the present invention, the concentration of the chloroauric acid solution is 12-15 g / L; the amount of the surface modifier added is 19.7 g / L-26.3 g / L; the amount of the reducing agent added is 100 g / L to 150 g / L; and the reducing agent is ascorbic acid.
[0013] As a preferred embodiment of the present invention, the glass powder comprises the following components in mass percentage: 10-20wt% calcium oxide, 10-25wt% boron oxide, and 55-80wt% silicon dioxide; the average particle size of the glass powder is less than 5 μm.
[0014] As a preferred embodiment of the present invention, the inorganic additive is one or more of zirconium oxide, zinc oxide, magnesium oxide and tin oxide.
[0015] As a preferred embodiment of the present invention, the organic carrier comprises resin, solvent and additives; the mass of the resin accounts for 5-10wt% of the mass of the organic carrier; the mass of the solvent accounts for 85-94wt% of the mass of the organic carrier; and the additives account for 1-5wt% of the mass of the organic carrier.
[0016] As a preferred embodiment of the present invention, the resin is one or more of cellulose, polyvinyl butyral, polyester, polyvinyl acetate, acrylate, p-tert-octyl phenolic resin, butyral resin, polyhexyl ethanol, poly-a-methylstyrene, and polyhexyl acetate; the solvent is one or more of terpineol, diethylene glycol monobutyl ether, n-butanol, butyl cellosolve acetate, benzyl alcohol, ethyl acetate, methyl ethyl ketone, butyl carbenzyl alcohol, isophorone, and heptane; the additive is one or more of Span 85, lecithin, lanolin, castor oil, dibutyl phthalate, and tributyl citrate.
[0017] As a preferred embodiment of the present invention, the method for preparing the organic carrier comprises the following steps: adding a portion of resin to the solvent, then heating to 79-100° C., adding another portion of resin to completely dissolve it, and then adding additives and stirring to obtain the organic carrier.
[0018] A method for printing and sintering low-temperature co-fired gold paste on a substrate, comprising: printing the low-temperature co-fired gold paste on a green ceramic sheet, and then laminating isostatic pressing and gradient sintering;
[0019] The lamination isostatic pressing process comprises: placing the green ceramic sheets with printed circuit patterns into a lamination mold according to the designed number of layers and order, the mold is designed with alignment columns consistent with the alignment holes of the green ceramic sheets to ensure alignment accuracy, then placing the stacked green ceramic bodies into a vacuum plastic bag, vacuuming and sealing, placing the packaged green ceramic bodies into hot water (temperature of 65-80° C.) in a pressure cylinder for preheating for 10-15 minutes, increasing the pressure to 21 MPa by a booster pump, and pressurizing for 15 minutes, so that the green ceramic bodies are evenly pressed and formed in the hot water;
[0020] The gradient sintering is specifically as follows: heating from room temperature to 100°C within 20-40 minutes, heating from 100°C to 200°C within 30-50 minutes, heating from 200°C to 300°C within 100-160 minutes, heating from 300°C to 450°C within 180-240 minutes, and then maintaining at 450°C for 10-15 minutes; continuing to heat from 450°C to 800°C within 60-80 minutes, heating from 800°C to 850°C within 20-40 minutes, and maintaining at 850°C for 18-20 minutes; then cooling to 800°C within 10-20 minutes, cooling from 800°C to 650°C within 15-35 minutes, cooling from 650°C to 500°C within 10-15 minutes, and finally cooling to room temperature for 3 hours to obtain the sintered gold paste.
[0021] The present invention can better control the shrinkage rate during the sintering process, reduce internal stress, reduce the warping and cracking of the substrate, and improve the flatness and mechanical strength of the substrate by strictly controlling the sintering gradient. It also helps to achieve a more uniform microstructure, reduce pores and defects, and improve the dielectric properties of the substrate, including dielectric constant and dielectric loss. In addition, gradient sintering can reduce thermal shock, improve the durability of the electronic components to be treated, and gradient sintering can shorten the sintering cycle, improve production efficiency, and maintain or improve product quality.
[0022] Compared with the prior art, the invention has the following beneficial effects: by controlling the morphology of gold powder, the invention prepares a low-temperature co-fired gold paste with high thixotropy, good plasticity, good conductivity, and excellent printing resolution; when inspected by bottom light, the lines are opaque, large-area metal is translucent, the co-firing matching is good, there are no cracks during sintering, the warpage of the substrate after sintering is less than 0.1 mm, the weldability is good, the welding resistance is good, and the application is wide, and the paste can be used for LTCC inner layer gold paste, LTCC surface layer gold paste, LTCC hole filling paste, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the SEM image of the gold powder prepared in Example 1.
[0024] Figure 2 This is a surface morphology diagram of the low-temperature co-fired gold paste prepared in Example 1 after printing on the SD-1 ceramic film.
[0025] Figure 3 This is a surface morphology diagram of the low-temperature co-fired gold paste prepared in Example 1 after sintering on the SD-1 ceramic film.
[0026] Figure 4 The morphology of the ceramic after sintering the low-temperature co-fired gold paste prepared in Example 1 on the raw ceramic film of SD-1, a is the morphology of the printed surface of the substrate, and b is the morphology of the printed back side of the substrate.
[0027] Figure 5 This is a SEM image of the surface after the low-temperature co-fired gold paste prepared in Example 1 was printed on the SD-1 ceramic film and sintered. DETAILED DESCRIPTION
[0028] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0029] Example 1
[0030] The preparation method of gold powder includes: dripping ammonia water into 15g / L chloroauric acid solution at a speed of 7mL / min and stirring, adjusting the pH to 7, and obtaining a fulminate gold solution. Concentrated hydrochloric acid is added to the fulminate gold solution at a speed of 4ml / min, adjusting the pH to 2, and adding 19.7g / L hexadecyltrimethylammonium bromide under mechanical stirring. After sufficient stirring, a reducing agent of 100g / L ascorbic acid is quickly added, and the reaction is carried out for 1h to obtain a reaction solution containing gold powder. The reaction solution containing gold powder is allowed to stand, and the gold powder that is precipitated by standing is washed and dried to obtain gold powder. Figure 1 It can be seen that the gold powder is a mixture of hexagonal flakes and spheres, with a purity of ≥99.95% and an average particle size of less than 10 μm.
[0031] The preparation method of glass powder includes: placing 15wt% calcium oxide, 15wt% boron oxide and 70wt% silicon dioxide in a platinum crucible, melting at 1500°C for 2 hours, and then pouring into deionized water for rapid water quenching to obtain glass slag. The glass slag is placed in a 90°C oven for drying for 2 hours, and then ball milled at a ball-to-material ratio of 4:1 to obtain D50=2-5μm glass powder; the average particle size of the glass powder is less than 5μm.
[0032] The preparation method of the organic carrier includes: adding 3wt% cellulose to 88wt% pineol, then heating to 90°C, stirring for 2h, then adding 5% cellulose and stirring until the resin is completely dissolved, and then adding 4wt% lanolin and stirring to obtain the organic carrier.
[0033] A method for preparing low-temperature co-fired gold paste comprises: adding 2.3% of glass powder and 1.7% of inorganic additive zirconium oxide to 20% of an organic carrier and fully dispersing them; then adding 76% of gold powder, rolling it through a three-roll mill for 15 times, filtering it through a 400-mesh screen, and obtaining the low-temperature co-fired gold paste.
[0034] A method for isostatic pressing and sintering after low-temperature co-fired gold paste printing and lamination, comprising: printing the above-mentioned gold paste mesh pattern on an SD-1 ceramic film, the size of the ceramic film is 101.6mm×101.6mm, and placing the raw ceramic sheets with printed circuit patterns into a lamination mold according to the designed number of layers and order. The mold is designed with alignment columns that are consistent with the alignment holes of the raw ceramic sheets to ensure alignment accuracy. The stacked raw ceramic body is placed in a vacuum plastic bag and vacuum-sealed. The packaged raw ceramic body is placed in hot water (temperature is 80°C) in a pressure cylinder for preheating for 15 minutes, pressurized to 21Mpa by a booster pump, and pressurized for 15 minutes, so that the raw ceramic body is evenly pressurized and formed in the hot water. Finally, the sintering curve is set for temperature-raising sintering. The sintering curve is as follows: the sintering temperature curve is to increase the temperature from room temperature to 100°C within 30 minutes, to increase the temperature from 100°C to 200°C within 35 minutes, to increase the temperature from 200°C to 300°C within 120 minutes, to increase the temperature from 300°C to 450°C within 200 minutes, and then maintain at 450°C for 10 minutes; continue to increase the temperature from 450°C to 800°C within 70 minutes, to increase the temperature from 800°C to 850°C within 30 minutes, and to maintain at 850°C for 18 minutes; then cool down to 800°C within 20 minutes, to cool down from 800°C to 650°C within 30 minutes, to cool down from 650°C to 500°C within 10 minutes, and finally cool down to room temperature for 3 hours to obtain the sintered gold paste. The prepared gold paste matches the sintering shrinkage rate of the ceramic film, the paste does not corrode the ceramic film, does not diffuse on the ceramic film after printing, has no cracks after sintering, has a warpage of less than 0.03mm, and has a square resistance of 2.4mΩ / sq.
[0035] Example 2
[0036] The preparation method of gold powder comprises: dripping ammonia water into 12g / L chloroauric acid solution at a speed of 8mL / min and stirring, adjusting the pH to 8, and obtaining a fulminate gold solution. Concentrated hydrochloric acid is added to the fulminate gold solution at a speed of 5ml / min, adjusting the pH to 1, and adding 26.3g / L 11-mercaptoundecanoic acid under mechanical stirring. After sufficient stirring, a reducing agent of 150g / L ascorbic acid is quickly added, and the reaction is carried out for 1h to obtain a reaction solution containing gold powder. The reaction solution containing gold powder is allowed to stand, and the gold powder that is precipitated by standing is washed and dried to obtain gold powder. The gold powder is a mixture of hexagonal flakes and spheres, with a purity of ≥99.95% and an average particle size of less than 10μm.
[0037] The preparation method of glass powder includes: placing 10wt% calcium oxide, 25wt% boron oxide and 65wt% silicon dioxide in a platinum crucible, melting at 1500°C for 2 hours, and then pouring into deionized water for rapid water quenching to obtain glass slag. The glass slag is placed in a 90°C oven for drying for 2 hours, and then ball milled at a ball-to-material ratio of 4:1 to obtain D50=2-5μm glass powder; the average particle size of the glass powder is less than 5μm.
[0038] The preparation method of the organic carrier includes: adding 4wt% polyhexyl alcohol to 88wt% diethylene glycol monobutyl ether, then heating to 90°C, stirring for 2h, then adding 6% polyhexyl alcohol and stirring until the resin is completely dissolved, and then adding 2wt% dibutyl phthalate and stirring to obtain the organic carrier.
[0039] A preparation method of low-temperature co-fired gold paste comprises: adding 2% of glass powder and 2% of inorganic additive cadmium oxide to 20% of organic carrier, and fully dispersing; then adding 76% of gold powder, rolling 15 times through a three-roll mill, filtering through a 400-mesh screen, and obtaining low-temperature co-fired gold paste.
[0040] A method for isostatic pressing and sintering after low-temperature co-fired gold paste printing and lamination, comprising: printing the above-mentioned gold paste mesh pattern on an SD-1 ceramic film, the ceramic film size is 101.6mm×101.6mm, and placing the raw ceramic sheets with printed circuit patterns into a lamination mold according to the designed number of layers and order. The mold is designed with alignment columns that are consistent with the alignment holes of the raw ceramic sheets to ensure alignment accuracy. The stacked raw ceramic body is placed in a vacuum plastic bag and vacuum-sealed. The packaged raw ceramic body is placed in hot water (temperature is 65°C) in a pressure cylinder for preheating for 10 minutes, pressurized to 21Mpa by a booster pump, and pressurized for 15 minutes, so that the raw ceramic body is evenly pressurized and formed in the hot water. Finally, the sintering curve is set for temperature-raising sintering. The sintering curve is as follows: the sintering temperature curve is to increase the temperature from room temperature to 100°C within 20 minutes, to increase the temperature from 100°C to 200°C within 38 minutes, to increase the temperature from 200°C to 300°C within 125 minutes, to increase the temperature from 300°C to 450°C within 220 minutes, and then maintain at 450°C for 15 minutes; continue to increase the temperature from 450°C to 800°C within 75 minutes, to increase the temperature from 800°C to 850°C within 30 minutes, and to maintain at 850°C for 20 minutes; then cool down to 800°C within 20 minutes, to cool down from 800°C to 650°C within 25 minutes, to cool down from 650°C to 500°C within 15 minutes, and finally to cool down to room temperature for 3 hours to obtain the sintered gold paste. The prepared gold paste matches the sintering shrinkage rate of the ceramic film, the paste does not corrode the ceramic film, does not diffuse on the ceramic film after printing, has no cracks after sintering, has a warpage of less than 0.03 mm, and has a square resistance of less than 2.2 mΩ / sq.
[0041] Example 3
[0042] The preparation method of gold powder comprises: dripping ammonia water into 12g / L chloroauric acid solution at a speed of 8mL / min and stirring, adjusting the pH to 8, and obtaining a fulminate gold solution. Concentrated hydrochloric acid is added to the fulminate gold solution at a speed of 5ml / min, adjusting the pH to 1, and adding 23.0g / L polyacrylic acid under mechanical stirring. After sufficient stirring, a reducing agent of 150g / L ascorbic acid is quickly added, and the reaction is carried out for 1h to obtain a reaction solution containing gold powder. The reaction solution containing gold powder is allowed to stand, and the gold powder that is allowed to stand and precipitate is washed and dried to obtain gold powder. The gold powder is a mixture of hexagonal flakes and spheres, with a purity of ≥99.95% and an average particle size of less than 10μm.
[0043] The preparation method of the glass powder in this embodiment is the same as that in embodiment 1.
[0044] The preparation method of the organic carrier includes: adding 4wt% polyvinyl acetate to 85wt% n-butanol, then heating to 90°C, stirring for 2h, then adding 6% polyvinyl acetate and stirring until the resin is completely dissolved, and then adding 5wt% tributyl citrate and stirring to obtain the organic carrier.
[0045] A method for isostatic pressing and sintering after printing and laminating low-temperature co-fired gold paste, characterized in that it includes: adding 1% glass powder and 5% inorganic additive cadmium oxide to 14% organic carrier and fully dispersing; then adding 80% gold powder, rolling 15 times through a three-roll mill, filtering through a 400-mesh screen, and obtaining low-temperature co-fired gold paste.
[0046] A method for low temperature co-fired gold paste printed substrate comprises: printing the above gold paste mesh pattern on a SD-1 ceramic film, the ceramic film size is 101.6mm×101.6mm, and placing the raw ceramic sheets with printed circuit patterns into a stacking mold according to the designed number of layers and order. The mold is designed with alignment columns that are consistent with the alignment holes of the raw ceramic sheets to ensure alignment accuracy. The stacked raw ceramic body is placed in a vacuum plastic bag and vacuum-sealed. The packaged raw ceramic body is placed in hot water (temperature is 70°C) in a pressure cylinder for preheating for 12 minutes, pressurized to 21Mpa by a booster pump, and pressurized for 15 minutes, so that the raw ceramic body is evenly pressurized and formed in the hot water. Finally, the sintering curve is set for temperature-raising sintering. The sintering curve is as follows: the sintering temperature curve is from room temperature to 100°C within 40 minutes, from 100°C to 200°C within 30 minutes, from 200°C to 300°C within 160 minutes, from 300°C to 450°C within 180 minutes, and then maintained at 450°C for 15 minutes; continue to heat from 450°C to 800°C within 60 minutes, from 800°C to 850°C within 40 minutes, and maintain at 850°C for 20 minutes; then cool down to 800°C within 10 minutes, cool down from 800°C to 650°C within 35 minutes, cool down from 650°C to 500°C within 15 minutes, and finally cool down to room temperature for 3 hours to obtain the sintered gold paste. The gold paste is matched with the raw tape, does not corrode, does not diffuse, has no cracks after sintering, has a warpage of less than 0.03mm, and a square resistance of less than 3mΩ / sq.
[0047] Example 4
[0048] The preparation method of gold powder comprises: dripping ammonia water into 12g / L chloroauric acid solution at a speed of 8mL / min and stirring, adjusting the pH to 8, and obtaining a fulminate gold solution. Concentrated hydrochloric acid is added to the fulminate gold solution at a speed of 5ml / min, adjusting the pH to 1, and adding 19.7g / L hexadecyltrimethylammonium bromide and 11-mercaptoundecanoic acid under mechanical stirring. After sufficient stirring, a reducing agent of 150g / L ascorbic acid is quickly added, and the reaction is carried out for 1h to obtain a reaction solution containing gold powder. The reaction solution containing gold powder is allowed to stand, and the gold powder that is allowed to stand and precipitate is washed and dried to obtain gold powder. The gold powder is a mixture of hexagonal flakes and spheres, with a purity of ≥99.95% and an average particle size of less than 10μm.
[0049] The preparation method of the glass powder in this embodiment is the same as that in embodiment 1.
[0050] The preparation method of the organic carrier in this embodiment is the same as that in embodiment 1.
[0051] A method for preparing low-temperature co-fired gold paste comprises: adding 5% of glass powder and 1% of inorganic additive zirconium oxide to 21% of organic carrier, and fully dispersing them; then adding 73% of gold powder, rolling 15 times with a three-roll mill, filtering through a 400-mesh screen, and obtaining low-temperature co-fired gold paste.
[0052] A method for low temperature co-fired gold paste printed substrate comprises: printing the above gold paste mesh pattern on a SD-1 ceramic film, the ceramic film size is 101.6mm×101.6mm, and placing the raw ceramic sheets with printed circuit patterns into a stacking mold according to the designed number of layers and order. The mold is designed with alignment columns that are consistent with the alignment holes of the raw ceramic sheets to ensure alignment accuracy. The stacked raw ceramic body is placed in a vacuum plastic bag and vacuum-sealed. The packaged raw ceramic body is placed in hot water (temperature is 70°C) in a pressure cylinder for preheating for 12 minutes, pressurized to 21Mpa by a booster pump, and pressurized for 15 minutes, so that the raw ceramic body is evenly pressurized and formed in the hot water. The sintering curve is set to perform temperature-raising sintering, and the sintering curve is as follows: the sintering temperature curve is to increase the temperature from room temperature to 100°C within 30 minutes, to increase the temperature from 100°C to 200°C within 50 minutes, to increase the temperature from 200°C to 300°C within 100 minutes, to increase the temperature from 300°C to 450°C within 240 minutes, and then maintain at 450°C for 15 minutes; continue to increase the temperature from 450°C to 800°C within 80 minutes, to increase the temperature from 800°C to 850°C within 20 minutes, and to maintain at 850°C for 20 minutes; then cool down to 800°C within 10 minutes, to cool down from 800°C to 650°C within 15 minutes, to cool down from 650°C to 500°C within 15 minutes, and finally cool down to room temperature for 3 hours to obtain the sintered gold paste. The gold paste is matched with the raw tape, does not corrode, does not diffuse, has no cracks after sintering, has a warpage of less than 0.03mm, and a square resistance of 2.3mΩ / sq.
[0053] Comparative Example 1
[0054] The preparation method of gold powder comprises: dripping ammonia water into 15g / L chloroauric acid solution at a speed of 7mL / min and stirring, adjusting the pH to 7, and obtaining a fulminate gold solution. Concentrated hydrochloric acid is added to the fulminate gold solution at a speed of 4ml / min, adjusting the pH to 2, adding a reducing agent 100g / L ascorbic acid under mechanical stirring, and reacting for 1h to obtain a reaction solution containing gold powder. The reaction solution containing the gold powder is allowed to stand, and the gold powder that is precipitated by standing is washed and dried to obtain the gold powder. The gold powder is a mixture of spherical and irregular flakes, and is severely agglomerated, with a purity of <95% and a wide particle size distribution.
[0055] The preparation method of the glass powder in this comparative example is the same as that in Example 1.
[0056] The preparation method of the organic carrier in this comparative example is the same as that in Example 1.
[0057] The preparation method of the low temperature co-fired gold paste in this comparative example is the same as that in Example 1.
[0058] The method for printing a substrate with low temperature co-fired gold paste in this comparative example is the same as that in Example 1.
[0059] Microscope inspection showed that the surface of the gold paste of Comparative Example 1 after sintering had bubbles and poor consistency, a warpage greater than 0.52 mm, and a square resistance greater than 0.5 mΩ / sq.
[0060] Comparative Example 2
[0061] The preparation method of the gold powder in this comparative example is the same as that in Example 1.
[0062] The preparation method of the glass powder in this comparative example is the same as that in Example 1.
[0063] The preparation method of the organic carrier in this comparative example is the same as that in Example 1.
[0064] The preparation method of the low temperature co-fired gold paste in this comparative example is the same as that in Example 1.
[0065] A method for low temperature co-firing gold paste printed substrate is as follows: the above gold paste mesh pattern is printed on a SD-1 ceramic film, the size of the ceramic film is 101.6mm×101.6mm, and the green ceramic sheets with printed circuit patterns are placed in a stacking mold according to the designed number of layers and order. The mold is designed with alignment columns consistent with the alignment holes of the green ceramic sheets to ensure alignment accuracy. The stacked green ceramic body is placed in a vacuum plastic bag and vacuum-sealed. The packaged green ceramic body is placed in hot water (temperature 70°C) in a pressure cylinder for preheating for 12 minutes, pressurized to 21Mpa by a booster pump, and pressurized for 15 minutes, so that the green ceramic body is uniformly pressed and formed in hot water. Sintering is performed according to the sintering curve, and the sintering curve is: heating to 450°C takes 120 minutes, heating to 850°C takes 120 minutes, and maintaining for 20 minutes, and then directly cooling.
[0066] Microscopic examination showed that the gold paste ceramic after sintering in Comparative Example 2 was warped, had an uneven surface, had a warpage greater than 0.71 mm, and had a square resistance greater than 0.4 mΩ / sq.
[0067] Comparative Example 3
[0068] The preparation method of gold powder comprises: dripping ammonia water into 15g / L chloroauric acid solution at a speed of 7mL / min and stirring, adjusting the pH to 7, and obtaining a fulminate gold solution. Concentrated hydrochloric acid is added to the fulminate gold solution at a speed of 4ml / min, adjusting the pH to 2, and adding 19.7g / L octadecyldimethylbenzyl quaternary ammonium chloride under mechanical stirring. After sufficient stirring, a reducing agent 100g / L ascorbic acid is quickly added, and the reaction is carried out for 1h to obtain a reaction solution containing gold powder. The reaction solution containing the gold powder is allowed to stand, and the gold powder that is allowed to stand and precipitate is washed and dried to obtain the gold powder. The gold powder is irregularly lamellar and exhibits an agglomerated form, with a purity of <96% and a wide particle size distribution.
[0069] The preparation method of the glass powder in this comparative example is the same as that in Example 1.
[0070] The preparation method of the organic carrier in this comparative example is the same as that in Example 1.
[0071] The preparation method of the low temperature co-fired gold paste in this comparative example is the same as that in Example 1.
[0072] The method for printing a substrate with low temperature co-fired gold paste in this comparative example is the same as that in Example 1.
[0073] Microscope inspection showed that the surface of the gold paste of Comparative Example 3 after sintering had bubbles and poor consistency, a warpage greater than 0.4 mm, and a square resistance greater than 0.4 mΩ / sq.
[0074] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A low temperature co-fired gold paste, characterized in that: The raw materials include the following weight percentages: 73-80 wt% gold powder, 1-5 wt% glass powder, 1-5 wt% inorganic additives, and 10-25 wt% organic carrier; The preparation method of the gold powder comprises the following steps: adding ammonia water to a chloroauric acid solution to adjust the pH to 7-8 to obtain a fulminate gold solution; adding concentrated hydrochloric acid to the fulminate gold solution to adjust the pH to 1-2, then adding a surface modifier and stirring, and then adding a reducing agent to react to obtain a reaction solution containing gold powder; and allowing the reaction solution to stand, separate, wash, and dry to obtain the gold powder; The surface modifier is at least one of hexadecyltrimethylammonium bromide, 11-mercaptoundecanoic acid and polyacrylic acid.
2. The low temperature co-fired gold paste according to claim 1, characterized in that: The gold powder is a mixture of hexagonal flakes and spheres, with a purity of ≥99.95% and an average particle size of less than 20 μm.
3. The low temperature co-fired gold paste according to claim 1, characterized in that: The concentration of the chloroauric acid solution is 12-15 g / L; the mass concentration of the surface modifier is 19.7 g / L-26.3 g / L; the mass concentration of the reducing agent is 100-150 g / L; and the reducing agent is ascorbic acid.
4. The low temperature co-fired gold paste according to claim 1, characterized in that: The inorganic additive is one or more of zirconium oxide, zinc oxide, magnesium oxide and tin oxide.
5. The low temperature co-fired gold paste according to claim 1, characterized in that: The glass powder comprises the following components in percentage by weight: 10-20 wt % of calcium oxide, 10-25 wt % of boron oxide and 55-80 wt % of silicon dioxide; the average particle size of the glass powder is less than 5 μm.
6. The low temperature co-fired gold paste according to claim 1, characterized in that: The organic carrier comprises the following components in percentage by weight: 5-10 wt % of resin, 85-94 wt % of solvent and 1-5 wt % of additive.
7. The low temperature co-fired gold paste according to claim 6, characterized in that: The resin is one or more of cellulose, polyvinyl butyral, polyester, polyvinyl acetate, acrylate, p-tert-octyl phenolic resin, butyral resin, polyhexyl alcohol, poly-a-methylstyrene, and polyhexyl acetate; the solvent is one or more of terpineol, diethylene glycol monobutyl ether, n-butanol, butyl cellosolve acetate, benzyl alcohol, ethyl acetate, methyl ethyl ketone, butyl carbenzyl alcohol, isophorone, and heptane; the additive is one or more of Span 85, lecithin, lanolin, castor oil, dibutyl phthalate, and tributyl citrate.
8. The low temperature co-fired gold paste according to claim 6, characterized in that: The method for preparing the organic carrier comprises the following steps: adding a portion of resin into a solvent, then heating it to 79-100° C., adding another portion of resin to completely dissolve it, and then adding an additive and stirring to obtain the organic carrier.
9. The method for preparing low temperature co-fired gold paste according to claim 1, characterized in that: The method comprises the following steps: mixing an organic carrier, glass powder and an inorganic additive; then adding gold powder, rolling through a three-roller rolling mill, filtering through a sieve, and obtaining a low-temperature co-fired gold paste.
10. A method for printing and sintering low temperature co-fired gold paste on a substrate, characterized in that: include: Printing the low temperature co-fired gold paste according to any one of claims 1 to 8 on a green ceramic sheet, followed by isostatic pressing and gradient sintering; The lamination isostatic pressing process specifically includes: placing the printed green ceramic sheets according to the designed number of layers and order, and then packaging, preheating and pressurizing the laminated green ceramic body under vacuum; The gradient sintering is specifically as follows: heating from room temperature to 100°C within 20-40 minutes, heating from 100°C to 200°C within 30-50 minutes, heating from 200°C to 300°C within 100-160 minutes, heating from 300°C to 450°C within 180-240 minutes, and then maintaining at 450°C for 10-15 minutes; continuing to heat from 450°C to 800°C within 60-80 minutes, heating from 800°C to 850°C within 20-40 minutes, and maintaining at 850°C for 18-20 minutes; then cooling to 800°C within 10-20 minutes, cooling from 800°C to 650°C within 15-35 minutes, cooling from 650°C to 500°C within 10-15 minutes, and finally cooling to room temperature for 3 hours to obtain the sintered gold paste.